MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
409 Stainless Steel
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel; T 400 Series Stainless Steel

Material Notes: Titanium content ranges from 6 times C content to 0.75%. One of least expensive of stainless steels.

Applications: mufflers, exterior parts, non-critical corrosive applications.

Key Words: UNS S40900, ASME SA268, ASTM A176, ASTM A268, ASTM A651, SAE J405 (51409), DIN 1.4512, JIS SUH 409, B.S. 409 S 17, ferritic, ISO 4954 X6CrNb12, ISO 683/13 1Ti
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 7.80 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 448 MPa
 30.0 MPa
@Temperature 870 °C
 61.0 MPa
@Temperature 760 °C
 148 MPa
@Temperature 650 °C
 254 MPa
@Temperature 540 °C
 326 MPa
@Temperature 425 °C
 334 MPa
@Temperature 315 °C
 365 MPa
@Temperature 205 °C
 406 MPa
@Temperature 93.0 °C
Tensile Strength, Yield 238 MPa
@Strain 0.2 %
 19.0 MPa
@Strain 0.2 %,
Temperature 870 °C
 39.0 MPa
@Strain 0.2 %,
Temperature 760 °C
 92.0 MPa
@Strain 0.2 %,
Temperature 650 °C
 136 MPa
@Strain 0.2 %,
Temperature 540 °C
 165 MPa
@Strain 0.2 %,
Temperature 425 °C
 172 MPa
@Strain 0.2 %,
Temperature 205 °C
 172 MPa
@Strain 0.2 %,
Temperature 315 °C
 207 MPa
@Strain 0.2 %,
Temperature 93.0 °C
Elongation at Break 32.5 %in 50 mm
 21 %
@Temperature 425 °C
in 50 mm
 22.5 %
@Temperature 315 °C
in 50 mm
 24 %
@Temperature 540 °C
in 50 mm
 25.5 %
@Temperature 205 °C
in 50 mm
 29.5 %
@Temperature 93.0 °C
in 50 mm
 44 %
@Temperature 650 °C
in 50 mm
 67.5 %
@Temperature 760 °C
in 50 mm
 75.5 %
@Temperature 870 °C
in 50 mm
Modulus of Elasticity 200 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000600 ohm-cm
@Temperature 20.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.7 µm/m-°C
@Temperature 20.0 - 100 °C
 11.9 µm/m-°C
@Temperature 20.0 - 260 °C
 12.4 µm/m-°C
@Temperature 20.0 - 480 °C
 12.9 µm/m-°C
@Temperature 20.0 - 650 °C
 13.5 µm/m-°C
@Temperature 20.0 - 815 °C
Specific Heat Capacity 0.460 J/g-°C
@Temperature 0.000 - 100 °C
Thermal Conductivity 24.9 W/m-K
@Temperature 95.0 °C
 28.6 W/m-K
@Temperature 540 °C
Melting Point 1425 - 1510 °C
Solidus 1425 °C
Liquidus 1510 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.080 %
Chromium, Cr 11.13 %
Iron, Fe 86 %
Manganese, Mn <= 1.0 %
Phosphorus, P <= 0.045 %
Silicon, Si <= 1.0 %
Sulfur, S <= 0.045 %
Titanium, Ti 0.75 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
410 Stainless Steel
304 Stainless Steel
420 Stainless Steel
409 Stainless Steel, annealed sheet, strip, plate, bar
416 Stainless Steel

MQ409B / 12940

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.