MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

(Viewing data as-entered. Click here to return)
DSM Somos® PerFORM Stereolithography Polymer, UV Postcure
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer

Material Notes: Somos® PerFORM produces strong, stiff, high temperature resistant composite parts that are ideal for tooling and wind tunnel testing applications. With the lowest viscosity of any composite stereolithography material, parts made from Somos® PerFORM are faster to build, easier to post-process clean, possess superior sidewall quality and provide unmatched detail resolution. It is the ideal material for creating strong, stiff parts with excellent high heat resistance, including wind tunnel models for aerospace and automotive applications, as well as rapid tooling for injection molding.

Key Benefits:

  • Excellent detail resolution
  • Fast, easy processing & finishing
  • Superior high heat tolerance
Ideal Applications:
  • Tooling
  • Wind tunnel testing
  • High temperature testing
  • Electrical casings
  • Automotive housings

Information provided by DSM.

Vendors:
Proto3000 provides design tools, 3D printers, additive manufacturing processes, metrology technologies, high-performance materials, and part-finishing automation. Our ISO 9001:2015 additive manufacturing production facility offers 3D printing services, rapid prototyping services, and end-part production with HP MultiJet Fusion (MJF), FDM, SLA, SLS, Polyjet, DLP, metal binder jetting, BMD, and DMLS.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.61 g/ccLiquid
Water Absorption 0.2 %ASTM D570-98
Viscosity 1000 cP
@Temperature 30.0 °C
Liquid
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 94ASTM D2240-05
Tensile Strength, Ultimate 68.0 MPaASTM D638-10
Elongation at Break 1.1 %ASTM D638-10
Modulus of Elasticity 10.5 GPaASTM D638-10
Flexural Strength 120 MPaASTM D790-10
Flexural Modulus 10000 MPaASTM D790-10
Poissons Ratio 0.32ASTM D638-10
Izod Impact, Notched 17.0 J/mASTM D256-10
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 3.6
@Frequency 1e+6 Hz
ASTM D150-11
 3.8
@Frequency 1000 Hz
ASTM D150-11
 4.0
@Frequency 60 Hz
ASTM D150-11
Dielectric Strength 26.3 kV/mmASTM D149-09
 
Thermal PropertiesOriginal ValueComments
CTE, linear 29.9 µm/m-°C
@Temperature -40.0 - 0.000 °C
ASTM E831-12
 49.4 µm/m-°C
@Temperature 0.000 - 50.0 °C
ASTM E831-12
 79.1 µm/m-°C
@Temperature 50.0 - 100 °C
ASTM E831-12
 80.9 µm/m-°C
@Temperature 100 - 150 °C
ASTM E831-12
Deflection Temperature at 0.46 MPa (66 psi) 132 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 82.0 °CASTM D648
Glass Transition Temp, Tg 72.0 °CASTM E1545-11
 
Descriptive Properties
AppearanceOff White
DP (mils)4.3Slope of cure-depth vs. ln (E) curve
E10 (mJ/cm2)80exposure that gives 0.254 mm (0.010 inch) thickness
Ec (mJ/cm2)7.8Critical Exposure

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DSM Somos® PerFORM Stereolithography Polymer, Thermal Postcure
DSM Somos® NanoTool™ Resin for Stereolithography, UV Postcure
DSM Somos® WaterShed® XC 11122 Water-resistant resin for stereolithography
3D Systems RenShape® SL 7820 Stereolithography Plastic
Aluminum A380.0-F Die Casting Alloy

PDSM9887c / 176054

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.