MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
IBC Advanced Alloys 41C Beryllium Nickel Casting Alloy
Categories: Metal; Nonferrous Metal; Beryllium Alloy; Nickel Alloy

Material Notes: Beryllium nickel casting alloys are characterized by their steel-like high strength, toughness, and hardness properties. However, unlike the steel alloys, the beryllium nickel alloy system offers these properties with the additional benefit of superior thermal conductivity. Beryllium nickel casting alloys are notable for their high resistance to wear, thermal shock, and corrosion even at elevated temperatures in the range of 1000°F (540°C).

The 40 series BeNiCr Casting Alloys have historically been utilized for high definition precision cast jewelry and commemorative rings, as well as, dental component applications.

Information provided by IBC Advanced Alloys.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.298 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 95 - 100Annealed
Hardness, Rockwell C 46 - 52Annealed and Aged
 
Thermal PropertiesOriginal ValueComments
CTE, linear 8.00 µin/in-°F
Melting Point 2100 - 2300 °F
Solidus 2100 °F
Liquidus 2300 °F
 
Processing PropertiesOriginal ValueComments
Casting Temperature 2300 - 2500 °FPouring Range
 
Component Elements PropertiesOriginal ValueComments
Beryllium, Be 2.5 - 2.85 %
Carbon, C 1.0 - 2.0 %
Chromium, Cr 0.45 - 0.80 %
Nickel, Ni 94.35 - 96.05 %As Balance

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
ASTM A485 Steel, Grade 1
Type 440B Martensitic Stainless Steel Bar, Tempered at 315°C, UNS S44003
AISI E51100 Steel
AISI 1095 Steel, oil quenched 800°C (1470°F), 595°C (1100°F) temper, 25 mm (1 in.) round
AISI 1095 Steel, oil quenched 800°C (1470°F), 480°C (900°F) temper, 100 mm (4 in.) round

NIBCA961 / 177696

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.