MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
EMS-Grivory Grilon® TS V0 PA666
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6/66

Material Notes: Product description: Grilon TS V0 is an unreinforced, normal viscosity, self-extinguishing Polyamid 66 + Polyamide 6 injection molding grade. Grilon TS V0 is halogen free and free of red phosphorous. The unpigmented material has a light inherent color.

RoHS: Grilon TS V0 is in compliance with RoHS (2002/95/EC, Restriction of hazardous Substances).

WEEE: Parts produced from Grilon TS V0 are not subject to “selective treatment” according the Directive 2002/96/EC on Waste Electrical and Electronic Equipment. Grilon TS V0 has the following important properties:

  • halogen free and free of red phosphorous.
  • UL-94 V0 at 0.4 mm wall thickness
  • High toughness
  • Suitable for molded Integral hinges
Grilon TS V0 is used typically for fuses, strips, cable binders, print terminals and coil former bobbins.

Information provided by EMS Grivory.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.16 g/ccDry; ISO 1183
Water Absorption 8.0 %Sim. to ISO 62
Moisture Absorption 2.50 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0070 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0080 cm/cmISO 294-4, 2577
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 50.0 MPaConditioned; ISO 527-1/-2
 75.0 MPaDry; ISO 527-1/-2
Tensile Strength, Yield 50.0 MPaConditioned; ISO 527-1/-2
 85.0 MPaDry; ISO 527-1/-2
Elongation at Break 10 %Nominal, Dry; ISO 527-1/-2
 >= 50 %Nominal, Conditioned; ISO 527-1/-2
Elongation at Yield 4.0 %Dry; ISO 527-1/-2
 15 %Conditioned; ISO 527-1/-2
Tensile Modulus 1600 MPaConditioned; ISO 527-1/-2
 3600 MPaDry; ISO 527-1/-2
Charpy Impact Unnotched 70.0 kJ/m²
@Temperature -30.0 °C
Dry; ISO 179/1eU
 75.0 kJ/m²
@Temperature 23.0 °C
Dry; ISO 179/1eU
 100 kJ/m²
@Temperature 23.0 °C
Conditioned; ISO 179/1eU
Charpy Impact, Notched 3.00 kJ/m²
@Temperature -30.0 °C
Dry; ISO 179/1eA
 3.00 kJ/m²
@Temperature -30.0 °C
Conditioned; ISO 179/1eA
 4.00 kJ/m²
@Temperature 23.0 °C
Dry; ISO 179/1eA
 15.0 kJ/m²
@Temperature 23.0 °C
Conditioned; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+9 ohm-cmConditioned; IEC 60093
 1.00e+11 ohm-cmDry; IEC 60093
Surface Resistance 1.00e+10 ohmIEC 60093
Dielectric Constant 3.0
@Frequency 1e+6 Hz
Dry; IEC 60250
 3.0
@Frequency 100 Hz
Dry; IEC 60250
 4.0
@Frequency 1e+6 Hz
Conditioned; IEC 60250
 8.0
@Frequency 100 Hz
Conditioned; IEC 60250
Dielectric Strength 26.0 kV/mmConditioned; IEC 60243-1
 28.0 kV/mmDry; IEC 60243-1
Dissipation Factor 0.0050
@Frequency 100 Hz
Dry; IEC 60250
 0.015
@Frequency 1e+6 Hz
Dry; IEC 60250
 0.070
@Frequency 1e+6 Hz
Conditioned; IEC 60250
 0.15
@Frequency 100 Hz
Conditioned; IEC 60250
Comparative Tracking Index 600 VConditioned; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 70.0 µm/m-°CISO 11359-1/-2
CTE, linear, Transverse to Flow 90.0 µm/m-°CISO 11359-1/-2
Melting Point 260 °C10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 100 - 120 °CLong Term; ISO 2578
 200 °CShort Term; EMS
Deflection Temperature at 0.46 MPa (66 psi) 210 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 70.0 °CISO 75-1/-2
Flammability, UL94 V-0IEC 60695-11-10
 V-0
@Temperature 1.50 °C
IEC 60695-11-10
Oxygen Index 35 %ISO 4589-1/-2
 
Descriptive Properties
AutomotiveAutomotive electr. and electronics, lighting
Electricals & ElectronicsCables & Tubes
 Connectors
 Electrical appliances
 Electrical equipment
 Energy distribution
 Lighting
FormGranules
ProcessingInjection Molding
Special CharacteristicsFlame retardant

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Ultramid® B24 N 03 PA6
Domo TECHNYL® 2411GF6 PA66, 30% glass fiber, DRY
EMS-Grivory Grilamid® L 20 EC PA12-CD25
EMS-Grivory Grilamid® XE 3817 black 9992 PA12
Domo TECHNYL® eXten D247 F Nylon 66 & 610

PGRH250 / 156959

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.