MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese Minlon® 73M40 NC010 PA6-MD40
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 40% Mineral Filled

Material Notes: 40% Mineral Reinforced Polyamide 6

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.45 g/ccDAM; ISO 1183
Melt Density 1.28 g/cc
@Temperature 270 °C
Water Absorption 5.4 %
@Thickness 2.00 mm
DAM; Sim. to ISO 62
Moisture Absorption 1.80 %
@Thickness 2.00 mm
DAM; Sim. to ISO 62
Viscosity Number 145 cm³/gsulfuric acid 96%; ISO 307, 1157, 1628
Linear Mold Shrinkage, Flow 0.0080 cm/cmDAM; ISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0080 cm/cmDAM; ISO 294-4, 2577
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 59.0 MPa50% RH; ISO 527-1/-2
 87.0 MPaDAM; ISO 527-1/-2
Elongation at Break 10 %DAM; ISO 527-1/-2
 25 %50% RH; ISO 527-1/-2
Tensile Modulus 2200 MPa50% RH; ISO 527-1/-2
 6000 MPaDAM; ISO 527-1/-2
Flexural Strength 60.0 MPa50% RH; ISO 178
 135 MPaDAM; ISO 178
Flexural Modulus 2400 MPa50% RH; ISO 178
 5900 MPaDAM; ISO 178
Poissons Ratio 0.35DAM
 0.3950% RH
Izod Impact, Notched (ISO) 4.00 kJ/m²
@Temperature -30.0 °C
DAM; ISO 180/1A
 4.50 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 180/1A
 5.00 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
 7.00 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 180/1A
Charpy Impact Unnotched 95.0 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 179/1eU
 95.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eU
 130 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eU
 NB
@Temperature 23.0 °C
50% RH; ISO 179/1eU
Charpy Impact, Notched 4.00 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eA
 5.00 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 179/1eA
 5.50 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 8.00 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 179/1eA
Tensile Creep Modulus, 1 hour 1400 MPa1h; 50% RH; ISO 899-1
Tensile Creep Modulus, 1000 hours 850 MPa1000h; 50% RH; ISO 899-1
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 65.0 µm/m-°CDAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow 75.0 µm/m-°CDAM; ISO 11359-1/-2
Specific Heat Capacity 1.94 J/g-°C
@Temperature 270 °C
Melt
Thermal Conductivity 0.270 W/m-K
@Temperature 270 °C
Melt
Melting Point 221 °C10°C/min; DAM; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 196 °CDAM; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 110 °CDAM; ISO 75-1/-2
Vicat Softening Point 210 °C50°C/h, 50N; DAM; ISO 306
Glass Transition Temp, Tg 70.0 °C10°C/min; DAM; ISO 11357-1/-2
Flammability, UL94 HB
@Thickness 0.850 mm
DAM; IEC 60695-11-10
 
Processing PropertiesOriginal ValueComments
Melt Temperature 270 °COptimum, Injection
 260 - 280 °CRange, Injection
Mold Temperature 70.0 - 120 °CInjection
 100 °COptimum, Injection
Ejection Temperature 210 °CInjection
Drying Temperature 80.0 °CInjection
Dry Time 2.00 - 4.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.20 %Injection
Hold Pressure 50.0 - 100 MPaInjection
 100 MPaInjection
 
Descriptive Properties
AdditivesRelease agent
Drying RecommendedyesInjection
FMVSS ClassSE/NBRISO 3795 (FMVSS 302)
Fogging (mg)0.15G-value (condensate); ISO 6452; DAM
ISO designationISO 16396-PA6,MD40,M1GHNR,S14-060
Max. screw tangential speed (m/s)0.2Injection
Odor Class3.5VDA 270
Part Marking Code>PA6-MD40<ISO 11469
PolymerPA6-MD40
Processing Hold Pressure Time (s/mm)3Injection
Resin IdentificationPA6-MD40ISO 1043
Thermal desorption analysis of organic emissions (µg/g)9VDA 270

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Envalior Durethan® BM 230 H2.0 901510 Nylon 6 (PA6), 30% Mineral Filled, Dry
Envalior Durethan® BM 230 H2.0 901510 Nylon 6 (PA6), 30% Mineral Filled, Conditioned
EMS-Grivory Grilon® BM-30 PA6-MD30
Celanese Minlon® 73M30 NC010 PA6-MD30
Celanese Zytel® 73G45L NC010 PA6-GF45

PDSX5251 / 197891

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.