MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
KKPC KOSYN 1500 Styrene Butadiene Rubber
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Styrene Butadiene Rubber

Characteristics: KOSYN SBR, a useful synthetic rubber, is a copolymer made from butadiene and styrene by cold emulsion polymerization. It has superior abrasion resistance and heat resistance in comparison with natural rubber, as well as widely useful physical properties of easy vulcanization and stable scorch properties. The products of KOSYN SBR are classified according to the emulsifying agent and stabilizer used in manufacturing process.

Applications: Tires, footwear, rubber hose, auto equipment and other rubber products for industrial use.

Additional Notes:
Bound Styrene: 23.5%
Stabilizer: Staining
Emulsifier: Rosin soap
Coagulant: Salt-Acid
Compound Properties: SRB 100, ZnO 3, S/A 1, HAF Black (IRB#7) 50, Accelerator TBBS1, Sulfur 1.75, Total: 156.75
Vulcanization: 145°C *35 m., Press Vulcanization

This product is so sensitive to sunlight and humidity that it can be tarnished and caused deterioration of quality if exposed. It is recommended to store it in cool and shady area lest it should be exposed to direct sunlight. Do not expose to incompatible materials or contaminants.

Data provided by Korea Kumho Petrochemical Co., Ltd.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.930 g/ccNot Compounded
Mooney Viscosity 52
@Temperature 100 °C
Raw; ML1+4
 80
@Temperature 100 °C
Compounded; ML1+4
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 71Vulcanized
Tensile Strength, Ultimate 302 kg(f)/cm²Vulcanized
Elongation at Break 500 %Vulcanized
300% Modulus 166 kg(f)/cm²
@Strain 300 %
Vulcanized
Rebound 55 %ASTM Test, Vulcanized
Flex Crack Resistance 34000145°C / 35 min., Press Vulcanization
Tear Strength 54.0 kg(f)/cmB-type, Vulcanized
Abrasion 0.20De Mattia Flexometer: Cut Growth 2mm --> 15mm, Flexes
Compression Set 51 %
@Temperature 100 °C
70 hrs, 25% def, Vulcanized

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
KKPC KOSYN 1507H Styrene Butadiene Rubber
DuPont Mobility and Materials Neoprene 750 Polychloroprene
Dow Buna® SB 1721 Cold polymerized Emulsion Styrene Butadiene Rubber (E-SBR)
Dow BETAPHON™ 2 Synthetic Rubber
Cri-Tech LS-715 FKM Fluoroelastomer, Durometer 70A

PKKPC00 / 48731

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.