MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Bedford Plastics Glass Reinforced Vinylester Flat Sheet, 3/8" to 1"
Categories: Polymer; Thermoset; Filled/Reinforced Thermoset; Vinyl Ester; Vinyl Ester Sheet Molding Compound

Material Notes: Flame retardant grade; see details in the property table.

Pultrusion results in the production and supply of one of the worlds strongest and most durable products available today. The pultruded products feature:

  • High Strength
  • Corrosion Resistant to many chemicals
  • Light Weight- Weighs nearly 80% less than a steel profile of similar dimension
  • Electrically Non-Conductive
  • Non-Metallic
  • Lower Life Cycle Cost
  • Non-Leaching. Environmentally Friendly
  • Dimensional Stability

Information provided by Bedford Plastics.

Key Words: Fiber Reinforced Plastic (FRP)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.72 - 1.94 g/cc0.0620 - 0.0700 lb/in³ASTM D792
Water Absorption <= 0.60 %<= 0.60 %24 hrs; ASTM D570
 
Mechanical PropertiesMetricEnglishComments
Hardness, Barcol 4040ASTM D2583
Tensile Strength, Ultimate 68.9 MPa10000 psiCrosswise; ASTM D638
 165 MPa24000 psiLengthwise; ASTM D638
Tensile Modulus 9.65 GPa1400 ksiCrosswise; ASTM D638
 13.8 GPa2000 ksiLengthwise; ASTM D638
Flexural Strength 124 MPa18000 psiCrosswise; ASTM D790
 207 MPa30000 psiLengthwise; ASTM D790
Flexural Modulus 9.65 GPa1400 ksiCrosswise; ASTM D790
 13.8 GPa2000 ksiLengthwise; ASTM D790
Compressive Strength 121 MPa17500 psiCrosswise; ASTM D635
 165 MPa24000 psiLengthwise; ASTM D635
Compressive Modulus 6.89 GPa1000 ksiCrosswise; ASTM D635
 12.4 GPa1800 ksiLengthwise; ASTM D635
Ultimate Bearing Strength 221 MPa32000 psiLengthwise; ASTM D953
Shear Strength 41.4 MPa6000 psiPerpendicular Shear Stress, Lengthwise; ASTM D3946
 41.4 MPa6000 psiPerpendicular Shear Stress, Crosswise; ASTM D3946
Izod Impact, Notched 2.67 J/cm5.00 ft-lb/inCrosswise; ASTM D256
 10.7 J/cm20.0 ft-lb/inLengthwise; ASTM D256
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength 1.38 kV/mm35.0 kV/inLengthwise; ASTM D149
 7.87 kV/mm200 kV/inPerpendicular to Laminate Face; ASTM D149
Arc Resistance 120 sec120 secLengthwise; ASTM D495
 
Thermal PropertiesMetricEnglishComments
CTE, linear 8.00 µm/m-°C
@Temperature 20.0 °C
4.44 µin/in-°F
@Temperature 68.0 °F
Lengthwise; ASTM D696
Flammability, UL94 V-0V-0
Flame Spread Index <= 25<= 25Tunnel Test; ASTM E84
Smoke Density 600 - 700600 - 700NBS; ASTM E662
 
Descriptive Properties
FlammabilityNonburningASTM D635

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Bedford Plastics Glass Reinforced FR Polyester Flat Sheet, 3/8" to 1"
Bedford Plastics Glass Reinforced Vinylester Flat Sheet, 1/8"
Bedford Plastics Glass Reinforced Vinylester Flat Sheet, 3/16" to 1/4"
Bedford Plastics Glass Reinforced Vinylester Structural Fiberglass Profiles
Quantum Composites QC-8805 66% Glass Fiber Vinyl Ester SMC

PBEDFO08 / 27105

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.