MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Teknor Apex Monprene® CP-11140 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Monprene CP-11100 High Density series of thermoplastic elastomer compounds, available in NAT or colors, from 40 to 90 Shore A, are designed specifically for consumer product applications requiring a soft, rubber-like feel. Monprene CP-11140 is a low hardness, high density, filled grade that is suitable for injection molding.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Features: Chemical Resistant; General Purpose; Good Adhesion; Good Colorability; Good Flexibility; Good Processability; High Density; Low Hardness; Low Specific Gravity

Uses: Appliances; Consumer Applications; Flexible Grips; Furniture; Handles; Household Goods; Knobs; Personal Care; Rubber Replacement; Safety Equipment; Soft Touch Applications; Sporting Goods; Stationary Supplies; Toys; Water Sports Equipment; Writing Instruments

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding

Preliminary data. Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.15 g/ccISO 1183
Viscosity 200 cP
@Shear Rate 206 1/s,
Temperature 200 °C
Capillary; ASTM D3835
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 40
@Time 5.00 sec
Injection Molded; ISO 868
Tensile Strength at Break 990 psiAcross Flow; ISO 37
Tensile Stress at Strain 95.0 psi
@Strain 100 %
Across Flow; ISO 37
Elongation at Break 950 %Across Flow; ISO 37
Tear Strength 80.0 pliAcross Flow; Method Ba, Angle (Unnicked); ISO 34-1
 100 pliFlow; Method Ba, Angle (Unnicked); ISO 34-1
Compression Set 26 %
@Temperature 70.0 °C,
Time 79200 sec
Type 1; ISO 815
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 320 - 350 °F
Middle Barrel Temperature 360 - 400 °F
Front Barrel Temperature 380 - 420 °F
Nozzle Temperature 360 - 440 °F
Melt Temperature 360 - 440 °F
Mold Temperature 80.0 - 120 °F
Back Pressure 25.0 - 100 psi
Cushion 0.150 - 0.500 in
Screw Speed 50 - 100 rpm
 
Descriptive Properties
AppearanceColors Available
 Opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PTEKNQ0769 / 237260

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.