MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Carpenter Thermo-Span® Fe-Co-Ni Superalloy
Categories: Metal; Superalloy; Iron Base

Material Notes: Data provided by Carpenter Technology Corporation.

Thermo-Span® alloy is a precipitation hardenable superalloy which exhibits a low coefficient of thermal expansion over a broad temperature range, high tensile and rupture strengths, and good thermal fatigue resistance. This alloy offers a significant improvement in environmental resistance over Pyromet® alloys CTX-1, CTX-3, AND CTX-909 due to the addition of chromium. the alloy also possesses an excellent combination of tensile properties and stress rupture strength in the recrystallized condition with the use of common solution and age hardening treatments. Unlike the CTX-family of alloys, the use of specific braze-cycle age hardening treatments is not required for Thermo-Span alloy due to the higher solution treating temperature.

Thermo-Span alloy should be considered for use in all applications for which the current low expansion superalloys are suited. These include compressor and exhaust casings, seals and other gas turbine components. Additional high temperature applications where moderate oxidation resistance is required are feasible with Thermo-Span alloy. This alloy should also be considered for use in applications requiring resistance to thermal fatigue.

Thermo-Span® is a registered trademark of Carpenter Technology Corporation.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.23 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 1227 MPa
 579 MPa
@Temperature 760 °C
 678 MPa
@Temperature 732 °C
 800 MPa
@Temperature 705 °C
 904 MPa
@Temperature 677 °C
 1055 MPa
@Temperature 649 °C
 1089 MPa
@Temperature 538 °C
 1175 MPa
@Temperature 260 °C
Tensile Strength, Yield 876 MPa
@Strain 0.2 %
 496 MPa
@Strain 0.2 %,
Temperature 760 °C
 579 MPa
@Strain 0.2 %,
Temperature 732 °C
 662 MPa
@Strain 0.2 %,
Temperature 705 °C
 745 MPa
@Strain 0.2 %,
Temperature 677 °C
 807 MPa
@Strain 0.2 %,
Temperature 538 °C
 814 MPa
@Strain 0.2 %,
Temperature 649 °C
 841 MPa
@Strain 0.2 %,
Temperature 260 °C
Elongation at Break 16 %In 4D
 15 %
@Temperature 538 °C
In 4D
 16 %
@Temperature 260 °C
In 4D
 19 %
@Temperature 677 °C
In 4D
 20 %
@Temperature 649 °C
In 4D
 24 %
@Temperature 705 °C
In 4D
 25 %
@Temperature 732 °C
In 4D
 30 %
@Temperature 760 °C
In 4D
Reduction of Area 32 %
 32 %
@Temperature 732 °C
 34 %
@Temperature 260 °C
 35 %
@Temperature 538 °C
 35 %
@Temperature 677 °C
 46 %
@Temperature 705 °C
 49 %
@Temperature 649 °C
 67 %
@Temperature 760 °C
Modulus of Elasticity 145 GPa
@Temperature 982 °C
 165 GPa
@Temperature 649 °C
 189 GPa
@Temperature 23.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 7.70 µm/m-°C
@Temperature 25.0 - 204 °C
 8.30 µm/m-°C
@Temperature 25.0 - 316 °C
 11.0 µm/m-°C
@Temperature 25.0 - 538 °C
Specific Heat Capacity 0.463 J/g-°C
@Temperature 23.0 °C
 0.518 J/g-°C
@Temperature 202 °C
 0.549 J/g-°C
@Temperature 652 °C
Thermal Conductivity 11.3 W/m-K
@Temperature 23.0 °C
 15.0 W/m-K
@Temperature 202 °C
 22.1 W/m-K
@Temperature 652 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 0.30 - 0.60 %
Boron, B <= 0.010 %
Carbon, C <= 0.050 %
Chromium, Cr 5.0 - 6.0 %
Cobalt, Co 28 - 30 %
Copper, Cu <= 0.50 %
Iron, Fe 34 %as remainder
Manganese, Mn <= 0.50 %
Nickel, Ni 23.5 - 25.5 %
Niobium, Nb (Columbium, Cb) 4.5 - 5.2 %
Phosphorus, P <= 0.015 %
Silicon, Si 0.20 - 0.30 %
Sulfur, S <= 0.015 %
Titanium, Ti 0.70 - 1.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Molded
Overview of materials for Acrylic, Cast
Aluminum, Al
Indium Corp. Indalloy 192 Pure Aluminum
Carpenter Pyromet® CTX-3 Superalloy, Heat Treated

NCARB0 / 15712

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.