MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Domo TECHNYL® B 50H1 Natural L PA 66/6, Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6/66; Nylon 66/6, Unreinforced

Material Notes: Description: TECHNYL® B 50H1 Natural L is an unreinforced melamine cyanurate flame retarded copolyamide 66/6. This product has been heat stabilized and is suitable for injection molding. This product is available in natural and other colors upon request.

Key Properties: UL94 V0 at 0.4mm; High ductility at low temperature; Excellent filling qualities

Benefits: This phosphorus and halogen free flame retardant grade, UL94 V0 at 0.4mm, offers excellent filling qualities together with good stiffness.

Applications: Connectivity : junction blocks, terminal blocks, connectors.

DOMO Chemicals has acquired Solvay’s Performance Polyamides Business in Europe.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.16 g/ccISO 1183/A
Water Absorption 1.1 %
@Time 86400 sec
ISO 62
Viscosity 20 cP
@Shear Rate 10000 1/s,
Temperature 280 °C
 20.1 cP
@Shear Rate 10000 1/s,
Temperature 270 °C
 20.2 cP
@Shear Rate 10000 1/s,
Temperature 260 °C
 220 cP
@Shear Rate 100 1/s,
Temperature 280 °C
 223 cP
@Shear Rate 100 1/s,
Temperature 270 °C
 224 cP
@Shear Rate 100 1/s,
Temperature 260 °C
Linear Mold Shrinkage 0.011 cm/cmIsotropy
Linear Mold Shrinkage, Flow 0.011 cm/cm
Linear Mold Shrinkage, Transverse 0.010 cm/cm
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 70.0 MPaISO 527 Type 1A
Tensile Strength, Yield 80.0 MPaISO 527 Type 1A
 85.0 MPaASTM D638
Tensile Stress at Strain 30.0 MPa
@Strain 1.5 %
 65.0 MPa
@Strain 2.5 %
 75.0 MPa
@Strain 3 %
 78.0 MPa
@Strain 4 %
Elongation at Break 10 %ISO 527 Type 1A
 10 %ASTM D638
Elongation at Yield 4.0 %ISO 527 Type 1A
Tensile Modulus 3600 MPaISO 527 Type 1A
Flexural Strength 105 MPaISO 178
 120 MPaASTM D790
Flexural Modulus 3650 MPaISO 178
Izod Impact, Unnotched 6.12 J/mASTM D256
Izod Impact, Notched (ISO) 5.00 kJ/m²ISO 180/1A
Charpy Impact Unnotched 90.0 kJ/m²ISO 179/1eU
Charpy Impact, Notched 4.50 kJ/m²ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmIEC 60093
Surface Resistance 1.00e+15 ohmIEC 60093
Dielectric Constant 3.6IEC 60250
Dielectric Strength 34.0 kV/mmIEC 60243
Dissipation Factor 0.020IEC 60250
Comparative Tracking Index 575 VSol B; IEC 60112
 600 VSol A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Transverse to Flow 60.0 µm/m-°C
@Temperature 23.0 - 85.0 °C
ISO 11359
Melting Point 242 °CISO 11357
Deflection Temperature at 1.8 MPa (264 psi) 85.0 °CISO 75/Af
Flammability, UL94 V-0
@Thickness 0.380 mm
ISO 1210
 V-0
@Thickness 0.800 mm
ISO 1210
 V-0
@Thickness 1.60 mm
ISO 1210
 V-0
@Thickness 3.20 mm
ISO 1210
Oxygen Index 33 %ISO 4589
Glow Wire Test 650 °C
@Thickness 1.60 mm
Ignition Temp; ISO 60695-2-13
 960 °C
@Thickness 0.800 mm
Flammability Index; ISO 60695-2-12
 960 °C
@Thickness 1.60 mm
Flammability Index; ISO 60695-2-12
 960 °C
@Thickness 3.20 mm
Flammability Index; ISO 60695-2-12
 
Processing PropertiesOriginal ValueComments
Processing Temperature 245 - 255 °CCompression zone
 250 - 260 °CMixing zone
Feed Temperature 240 - 250 °C
Mold Temperature 60.0 - 80.0 °C
Drying Temperature 80.0 °C
Moisture Content <= 0.20 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Domo TECHNYL® B 50H1 Natural L PA 66/6, Conditioned
Domo TECHNYL® B 50 H1 PA66/6, DRY
Domo Technyl® B 50H1 Nylon 66/6, Flame Retardant, EH50
Nilit Polynil® C50 PA66/6 Co-Polymer
Nilit Polynil® C50L Externally Lubricated PA66/6

PSOLVAY853 / 218581

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.