MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Americas Styrenics Styron® 692 Polystyrene
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene, Heat Resistant Grade

Material Notes: Product Characteristics:
  • High tensile strength
  • High stiffness
  • Food Contact Compliant
  • UL Classification 94 HB
Typical Applications:
  • Appliance parts
  • Housewares

Americas Styrenics was formed in 2008 as a joint venture between Dow Chemical and Chevron Phillips Chemical Company. Styron was a Dow trade name before the JV formation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.04 g/ccASTM Data
Linear Mold Shrinkage 0.00400 - 0.00800 cm/cm
Melt Flow 4.0 g/10 min
@Load 5.00 kg,
Temperature 200 °C
ASTM Data
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell L 109
Tensile Strength at Break 47.0 MPaASTM D638
Tensile Strength 6800 psiASTM D638
Elongation at Break 3.0 %ASTM D638
Tensile Modulus 450000 psiASTM D638
Flexural Strength 8.60 ksiASTM D790
Flexural Modulus 485000 psiASTM D790
Izod Impact, Notched 0.400 ft-lb/inASTM D256
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 50.0 µm/m-°C
@Temperature 23.0 °C
ASTM data
Deflection Temperature at 0.46 MPa (66 psi) 187 °CUnannealed; ASTM Data
Deflection Temperature at 1.8 MPa (264 psi) 175 °CUnannealed; ASTM Data
Vicat Softening Point 210 °C
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 213 - 243 °CInjection Molding
Zone 1 177 - 193 °CExtrusion Molding
 218 - 249 °CInjection Molding
Zone 2 182 - 204 °CExtrusion Molding
 218 - 249 °CInjection Molding
Zone 3 188 - 210 °CExtrusion Molding
 199 - 213 °CInjection Molding
Zone 4 199 - 216 °CExtrusion Molding
Zone 5 204 - 221 °CExtrusion Molding
Die Temperature 199 - 232 °CExtrusion Molding
Melt Temperature 193 - 232 °CExtrusion Molding
Back Pressure 25.0 - 175 MPaInjection Molding
 
Descriptive Properties
Head Pressure10-21 MPa
Melt Pump, Adapter, Pipes, Screen Changer193-232°C
Polish Rolls66-104°C
Zone # 6204-221°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PDW174_a / 323915

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.