MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Dow AFFINITY™ PF 1140G Polyolefin Plastomer (POP)
Categories: Polymer; Film; Thermoplastic; Polyolefin

Material Notes: AFFINITY™ PF 1140G is an ethylene alpha-olefin resin produced via INSITE™ Technologies. It is designed to be used in a variety of demanding applications including form-fill-seal packaging and fresh produce bags. This resin has excellent compatibility with other polyolefins, allowing efficient blending and co-extrusion.

Information provided by Dow

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.8965 g/ccASTM D792
Thickness 2.00 mil
Melt Flow 1.6 g/10 minASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Film Tensile Strength at Yield, MD 840 psiASTM D882
Film Tensile Strength at Yield, TD 920 psiASTM D882
Film Elongation at Break, MD 690 %ASTM D882
Film Elongation at Break, TD 700 %ASTM D882
Secant Modulus, MD 0.0730 GPa2% Secant; ASTM D882
Secant Modulus, TD 0.0730 GPa2% Secant; ASTM D882
Impact 18.8[lbf]; Puncture Resistance Force; Dow Method
 245[ft-lbf/in3]; Puncture Resistance; Dow Method
Puncture Energy 72.4 in-lbDow Method
Elmendorf Tear Strength MD 470 gModified rectangular test specimen; ASTM D1922
Elmendorf Tear Strength TD 620 gModified rectangular test specimen; ASTM D1922
Elmendorf Tear Strength, MD 235 g/milASTM D1922
Elmendorf Tear Strength, TD 310 g/milASTM D1922
Dart Drop Test >= 850 gMethod B; ASTM D1709
Film Tensile Strength at Break, MD 7290 psiASTM D882
Film Tensile Strength at Break, TD 5730 psiASTM D882
Heat Seal Strength Initiation Temperature 81.0 °C2 lb/in heat seal strength; 0.5 sec dwell, 40 psi bar pressure, pull speed 10 (in./min.); Dow Method
 
Thermal PropertiesOriginal ValueComments
Melting Point 96.0 °CDow Method (DSC)
Vicat Softening Point 77.0 °CASTM D1525
 
Optical PropertiesOriginal ValueComments
Haze 1.3 %ASTM D1003
Gloss 134 %20°; ASTM D2457
Transmission, Visible 70 %Clarity; ASTM D1746

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Dow AFFINITY™ GA 1900 Polyolefin Plastomer (POP)
Dow AFFINITY™ EG 8185 Polyolefin Plastomer (POP)
Dow AFFINITY™ EG 8200G Ethylene alpha-olefin copolymer
Dow AFFINITY™ GA 1950 Polyolefin Plastomer (POP)
Dow AFFINITY™ PL 1880G Polyolefin Plastomer (POP)

PDOW1171 / 30389

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.