MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

420 Stainless Steel, annealed bar
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel; T 400 Series Stainless Steel

Key Words: UNS S42000, AMS 5506, AMS 5621, ASTM A276, ASTM A314, ASTM A473, ASTM A580, FED QQ-S-763, FED QQ-S-766, FED QQ-W-423, MIL SPEC MIL-S-862, SAE J405 (51420), B.S. 420 S 37, B.S. CDS-18 (U.K), martensitic, DIN 1.4021, AFNOR Z 20 C 13 (Fr), UNI X 20 Cr 13, JIS SUS 420 J1, SS14 2303 (Sweden), ISO 683/13 4
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 195195
Hardness, Rockwell C 1212Converted from Brinell Hardness. Value below normal Rockwell C Hardness range, for comparison only.
Tensile Strength, Ultimate 655 MPa95000 psi
Tensile Strength, Yield 345 MPa
@Strain 0.2 %
50000 psi
@Strain 0.2 %
Elongation at Break 25 %25 %in 50 mm
Modulus of Elasticity 200 GPa29000 ksi
Poissons Ratio 0.240.24Calculated
Shear Modulus 80.7 GPa11700 ksi
Charpy Impact  14.0 J
@Temperature 23.0 °C
10.3 ft-lb
@Temperature 73.4 °F
 100 J
@Temperature 23.0 °C
73.8 ft-lb
@Temperature 73.4 °F
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000550 ohm-cm
@Temperature 20.0 °C
0.0000550 ohm-cm
@Temperature 68.0 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.3 µm/m-°C
@Temperature 0.000 - 100 °C
5.72 µin/in-°F
@Temperature 32.0 - 212 °F
 10.8 µm/m-°C
@Temperature 0.000 - 315 °C
6.00 µin/in-°F
@Temperature 32.0 - 599 °F
 11.7 µm/m-°C
@Temperature 0.000 - 540 °C
6.50 µin/in-°F
@Temperature 32.0 - 1000 °F
 12.2 µm/m-°C
@Temperature 0.000 - 650 °C
6.78 µin/in-°F
@Temperature 32.0 - 1200 °F
Specific Heat Capacity 0.460 J/g-°C
@Temperature 0.000 - 100 °C
0.110 BTU/lb-°F
@Temperature 32.0 - 212 °F
Thermal Conductivity 24.9 W/m-K
@Temperature 100 °C
173 BTU-in/hr-ft²-°F
@Temperature 212 °F
Melting Point 1455 - 1510 °C2651 - 2750 °F
Solidus 1455 °C2651 °F
Liquidus 1510 °C2750 °F
Maximum Service Temperature, Air 620 °C1150 °FContinuous Service
 735 °C1360 °FIntermittent
 
Component Elements PropertiesMetricEnglishComments
Carbon, C >= 0.15 %>= 0.15 %
Chromium, Cr 13 %13 %
Iron, Fe 85 %85 %
Manganese, Mn <= 1.0 %<= 1.0 %
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.030 %<= 0.030 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
420 Stainless Steel
420 Stainless Steel, hardened and tempered bar
420 Stainless Steel, annealed and cold drawn bar
430 Stainless Steel annealed bar
414 Stainless Steel, annealed and cold drawn bar

MQ420M / 13075

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.