MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Barlog Plastics KEBAFLEX H / SPBT 50 A.01 natural SEBS
Categories: Polymer; Thermoplastic; Elastomer, TPE; Styrenic TPE

Material Notes: TPE-S, Shore A50, natural, modified for good adhesion to PBT and PBT blends, among others.

Properties: flexible, good haptics, adhesion modified, High weather resistance, semi-crystalline, soft

Typical areas of application: Sealing elements, Seals, Spring elements, Handles, Haptic components

Industries: Automotive, Electrical and electronics industry, Household appliances, Industry, Mechanical Engineering, Furniture industry, Sports & Recreation

Information provided by BARLOG plastics GmbH.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.01 g/ccISO 1183-1
Linear Mold Shrinkage, Flow 0.0270 cm/cmISO 294-4
Linear Mold Shrinkage, Transverse 0.0150 cm/cmISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 48.0DIN ISO 7619-1
Tensile Strength at Break 5.00 MPaISO 527-1
Tensile Strength, Yield 0.500 MPa
@Strain 10.0 %
DIN EN ISO 527-1
Elongation at Break 700 %ISO 527-1
50% Modulus 1.20 MPa
@Strain 50.0 %
DIN EN ISO 527-1
100% Modulus 1.50 MPa
@Strain 100 %
DIN EN ISO 527-1
300% Modulus 2.70 MPa
@Strain 300 %
DIN EN ISO 527-1
Compression Set 67.0 %
@Treatment Temp. 70.0 °C
ISO 815-1
 83.0 %
@Treatment Temp. 100 °C
ISO 815-1
 
Processing PropertiesOriginal ValueComments
Melt Temperature 220 - 250 °C
Mold Temperature 20.0 - 40.0 °C
Drying Temperature 80.0 °C
Dry Time 3.00 - 4.00 hour
Moisture Content <= 0.0200 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PBARLO611 / 326685

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.