MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

DuPont Mobility and Materials Delrin® PC690 NC010 POM  (discontinued **)
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM)

Material Notes: Low Viscosity Acetal Homopolymer Developed for the Healthcare Industry

Information provided by DuPont; The Delrin product line was sold by DuPont in 2023 but this specific grade was discontinued prior to the sale

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.42 g/cc0.0513 lb/in³ISO 1183
Water Absorption 1.4 %
@Thickness 2.00 mm
1.4 %
@Thickness 0.0787 in
Sim. to ISO 62
Moisture Absorption 0.300 %
@Thickness 2.00 mm
0.300 %
@Thickness 0.0787 in
Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.019 cm/cm0.019 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.019 cm/cm0.019 in/inISO 294-4, 2577
Melt Flow 25 g/10 min25 g/10 minISO 1133
 21 g/10 min
@Load 2.16 kg,
Temperature 190 °C
21 g/10 min
@Load 4.76 lb,
Temperature 374 °F
cm³/10min Volumetric Rate; ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 9292ISO 2039-2
Hardness, Rockwell R 120120ISO 2039-2
Tensile Strength, Yield 71.0 MPa10300 psiISO 527-1/-2
Elongation at Break 23 %23 %ISO 527-1/-2
Elongation at Yield 12 %12 %ISO 527-1/-2
Tensile Modulus 3.30 GPa479 ksiISO 527-1/-2
Flexural Modulus 3.00 GPa435 ksiISO 178
Poissons Ratio 0.370.37ISO 527-1/-2
Izod Impact, Unnotched (ISO)  7.00 kJ/m²
@Temperature 23.0 °C
3.33 ft-lb/in²
@Temperature 73.4 °F
ISO 180/1A
 8.00 kJ/m²
@Temperature -40.0 °C
3.81 ft-lb/in²
@Temperature -40.0 °F
ISO 180/1A
Charpy Impact Unnotched  20.0 J/cm²
@Temperature 23.0 °C
95.2 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
 20.0 J/cm²
@Temperature -30.0 °C
95.2 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched  0.700 J/cm²
@Temperature -30.0 °C
3.33 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 0.800 J/cm²
@Temperature 23.0 °C
3.81 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
Tensile Creep Modulus, 1 hour 2800 MPa406000 psiISO 899-1
Tensile Creep Modulus, 1000 hours 1500 MPa218000 psiISO 899-1
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+14 ohm-cm1.00e+14 ohm-cmIEC 62631-3-1
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmIEC 62631-3-2
Dielectric Constant  3.8
@Frequency 1e+6 Hz
3.8
@Frequency 1e+6 Hz
IEC 62631-2-1
 3.8
@Frequency 100 Hz
3.8
@Frequency 100 Hz
IEC 62631-2-1
Comparative Tracking Index 600 V600 VIEC 60112
Hot Wire Ignition, HWI 8.0 sec
@Thickness 0.750 mm
8.0 sec
@Thickness 0.0295 in
UL 746A
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 120 µm/m-°C66.7 µin/in-°FISO 11359-1/-2
 104 µm/m-°C
@Temperature 23.0 - 55.0 °C
57.8 µin/in-°F
@Temperature 73.4 - 131 °F
ASTM E 831
CTE, linear, Transverse to Flow 120 µm/m-°C66.7 µin/in-°FISO 11359-1/-2
Melting Point 178 °C352 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 162 °C324 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 94.0 °C201 °FISO 75-1/-2
Vicat Softening Point 160 °C320 °F50°C/h, 50N; ISO 306
Oxygen Index 23 %23 %ASTM D 2863
 
Processing PropertiesMetricEnglishComments
Melt Temperature 210 - 220 °C410 - 428 °FInjection
 215 °C419 °FInjection Optimum
Mold Temperature 80.0 - 100 °C176 - 212 °FInjection
 90.0 °C194 °FInjection Optimum
Drying Temperature 80.0 °C176 °FInjection
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hourDehumidified Dryer; Injection
Moisture Content 0.20 %0.20 %Injection
Hold Pressure 80.0 - 100 MPa11600 - 14500 psiInjection
Annealing Temperature 160 °C320 °FInjection
 
Descriptive Properties
AdditivesLubricants
 Release agent
Annealing time30 min/mmInjection - Optional
Delivery formPellets
Drying RecommendedyesInjection
Emissions<8 mg/kgVDA 275
Fogging F-value (refraction) (%)95ISO 6452
Fogging G-value (condensate) (mg)0.2ISO 6452
Hold pressure time (s/mm)8Injection
Part Marking CodePOMISO 11469
ProcessingInjection Molding
Resin IdentificationPOMISO 1043

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Delrin® PC699 NC010 POM
Delrin Delrin® 900P NC010 POM
Delrin Delrin® 500AL NC010 POM-S
Delrin Delrin® 500CL NC010 POM
Delrin Delrin® FG900P NC010 POM

PDSX5158 / 197798

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.