MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Covestro Makrolon® 2408 Polycarbonate
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Molded

Material Notes: MVR (300 °C/1.2 kg) 19 cm³/10 min; medical devices; suitable for ETO and steam sterilization at 121 °C; biocompatible according to many ISO 10993-1 test requirements; low viscosity; injection molding - melt temperature 280 - 320 °C; available in color code 000000 only

As of 1 September 2015, Bayer MaterialScience was separated from Bayer AG and officially adopted its new name – Covestro.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Bulk Density 0.660 g/ccpellets; ISO 60
Density 1.20 g/ccISO 1183-1
Moisture Absorption at Equilibrium 0.12 %ISO 62, 50% RH
Water Absorption at Saturation 0.30 %ISO 62
Linear Mold Shrinkage, Flow 0.0065 cm/cm
@Thickness 2.00 mm
60x60x2 mm; 500 bar; ISO 294-4
Linear Mold Shrinkage, Transverse 0.0065 cm/cm
@Thickness 2.00 mm
60x60x2 mm; 500 bar; ISO 294-4
Melt Flow 20 g/10 min
@Load 1.20 kg,
Temperature 300 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Puncture Resistance 5100 N
@Temperature 23.0 °C
ISO 6603-2
 6000 N
@Temperature -30.0 °C
ISO 6603-2
Ball Indentation Hardness 113 MPaISO 2039-1
Tensile Strength at Break 70.0 MPa50 mm/min; ISO 527-1,-2
Tensile Strength, Yield 65.0 MPa50 mm/min; ISO 527-1,-2
Elongation at Break >= 50 %Nominal, 50 mm/min; ISO 527-1,-2
 120 %50 mm/min; b.o. ISO 527-1,-2
Elongation at Yield 6.3 %50 mm/min; ISO 527-1,-2
Tensile Modulus 2350 MPa1 mm/min; ISO 527-1,-2
Flexural Strength 96.0 MPa2 mm/min; ISO 178
Flexural Yield Strength 72.0 MPa
@Strain 3.5 %
2 mm/min; ISO 178
Flexural Modulus 2350 MPa2 mm/min; ISO 178
Flexural Strain at Yield 7.0 %2 mm/min; ISO 178
Izod Impact, Notched (ISO) 12.0 kJ/m²
@Thickness 3.00 mm,
Temperature -30.0 °C
complete break; b.o. ISO 180-A
 75.0 kJ/m²
@Thickness 3.00 mm,
Temperature 23.0 °C
partial break; b.o. ISO 180-A
Charpy Impact Unnotched NB
@Temperature 23.0 °C
ISO 179-1eU
 NB
@Temperature -30.0 °C
ISO 179-1eU
 NB
@Temperature -60.0 °C
ISO 179-1eU
Charpy Impact, Notched 14.0 kJ/m²
@Thickness 3.00 mm,
Temperature -30.0 °C
complete break; ISO 7391/b.o. ISO 179-1eA
 65.0 kJ/m²
@Thickness 3.00 mm,
Temperature 23.0 °C
partial break; ISO 7391/b.o. ISO 179-1eA
Puncture Energy 55.0 J
@Temperature 23.0 °C
ISO 6603-2
 65.0 J
@Temperature -30.0 °C
ISO 6603-2
Tensile Creep Modulus, 1 hour 2200 MPaISO 899-1
Tensile Creep Modulus, 1000 hours 1900 MPaISO 899-1
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 65.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
CTE, linear, Transverse to Flow 65.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
Thermal Conductivity 0.200 W/m-Kcross-flow; ISO 8302
Hot Ball Pressure Test 138 °CIEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 139 °CISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi) 127 °CISO 75-1,-2
Vicat Softening Point 147 °C
@Load 5.10 kg
50°C/h; ISO 306
 148 °C
@Load 5.10 kg
120°C/h; ISO 306
Glass Transition Temp, Tg 147 °C10°C/min; ISO 11357-1,-2
Flash Point 480 °CASTM D 1929
 550 °Cself ignition; ASTM D 1929
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.586Procedure A; ISO 489
Haze <= 0.80 %
@Thickness 3.00 mm
ISO 14782
Transmission, Visible 87 %
@Thickness 4.00 mm
ISO 13468-2
 88 %
@Thickness 3.00 mm
ISO 13468-2
 89 %
@Thickness 1.00 mm
ISO 13468-2
 89 %
@Thickness 2.00 mm
ISO 13468-2
 
Processing PropertiesOriginal ValueComments
Melt Temperature 280 °CInjection molding; ISO 294
Mold Temperature 80.0 °CInjection molding; ISO 294
Injection Velocity 200 mm/secISO 294

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Covestro Makrolon® 2258 Polycarbonate
Covestro Makrolon® 2405 MAS048 Polycarbonate
Covestro Makrolon® 1954 Polycarbonate
Overview of materials for Polycarbonate, Molded
Covestro Makrolon® 2407 MAS070 Polycarbonate

PB09617 / 150749

USP Class VI adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.