MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Titanium IMI 834
Categories: Metal; Nonferrous Metal; Titanium Alloy; Alpha/Near Alpha Titanium Alloy

Material Notes: Heat Treatment: 1015ºC 2 hr; oil quench; 700ºC 2 hr; air cool.

Characteristics: Near-alpha alloy, mid-range strength, good elevated temperature properties, good fatigue resistance.

Applications: Aerospace - compressor discs and blades.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 4.55 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 326Estimated from Rockwell C.
Hardness, Knoop 354Estimated from Rockwell C.
Hardness, Rockwell C 35
Hardness, Vickers 350
Tensile Strength, Ultimate 1050 MPa
Tensile Strength, Yield 925 MPa
Elongation at Break 12 %
Reduction of Area 15 %
Modulus of Elasticity 120 GPa
Poissons Ratio 0.31Typical for alpha titanium alloy.
Fatigue Strength 340 MPa
@# of Cycles 1.00e+7
kt = 2.0, wrought 50 mm diameter bar.
 530 MPa
@# of Cycles 400000
kt = 2.0, heat treated bar, axial stress
 530 MPa
@# of Cycles 1.00e+7
Unnotched
 900 MPa
@# of Cycles 10000
heat treated bar, axial stress, Unnotched
Fracture Toughness 45.0 MPa-m½
Shear Modulus 45.8 GPaCalculated from typical values.
Charpy Impact 15.0 JV-notch
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000160 ohm-cmEstimated from similar alpha titanium alloys.
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.6 µm/m-°C
@Temperature 20.0 - 200 °C
 10.9 µm/m-°C
@Temperature 20.0 - 400 °C
average
 11.0 µm/m-°C
@Temperature 20.0 - 600 °C
average
 11.3 µm/m-°C
@Temperature 20.0 - 1000 °C
Specific Heat Capacity 0.525 J/g-°CTypical value for titanium alloys.
Thermal Conductivity 7.00 W/m-KEstimated from similar titanium alloys.
Beta Transus 1045 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 5.8 %
Molybdenum, Mo 0.50 %
Niobium, Nb (Columbium, Cb) 0.70 %
Silicon, Si 0.35 %
Tin, Sn 4.0 %
Titanium, Ti 85 %
Zirconium, Zr 3.5 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Titanium IMI 829 (Ti-5.5Al-3.5Sn-3Zr-1Nb-0.25Mo-0.3Si)
Titanium IMI 685 (Ti-6Al-5Zr-0.5Mo-0.25Si)
Titanium Ti-6Al-2Sn-4Zr-2Mo-0.1Si; Duplex Annealed
Titanium, Ti
Titanium Ti-6Al-4V (Grade 5), Annealed

MTA832 / 14142

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.