MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Carmel Olefins Ipethene® 322 Low Density Polyethylene
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Low Density (LDPE); Low Density Polyethylene (LDPE), Extrusion Grade

Material Notes: IPETHENE® 322 is a general purpose low density polyethylene film extrusion grade. It contains a medium level of anti-blocking and slip additives. It is BHT free. It exhibits a good balance between mechanical and optical properties.

APPLICATIONS

IPETHENE® 322 is mainly used for the production of 25 to 80 µm films for general purposes and Form-Fill-Seal packaging.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.920 g/ccISO 1183-A
Thickness 50.0 microns
Melt Flow 2.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Film Elongation at Break, MD 230 %ISO 1184
Film Elongation at Break, TD 500 %ISO 1184
Elmendorf Tear Strength MD 600 gISO 6283-2
Elmendorf Tear Strength TD 250 gISO 6283-2
Elmendorf Tear Strength, MD 12.0 g/micronISO 6283-2
Elmendorf Tear Strength, TD 5.00 g/micronISO 6283-2
Dart Drop 2.50 g/micronF50; ISO 7765-A
Dart Drop Test 125 gF50; ISO 7765-A
Film Tensile Strength at Break, MD 22.0 MPaISO 1184
Film Tensile Strength at Break, TD 15.0 MPaISO 1184
 
Optical PropertiesOriginal ValueComments
Haze 6.0 %ASTM D1003
Gloss 65 %45°; ASTM D2457
 
Processing PropertiesOriginal ValueComments
Melt Temperature 160 °C
Blow-up Ratio (BUR) 2.0

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Kazanorgsintez 107-22 Composition of Low Density Polyethylene, Crack-Proof
LG Chemical SEETEC BF500 LDPE
Carmel Olefins Ipethene® 320 Low Density Polyethylene
Dow LDPE 4005 Low Density Polyethylene, Extrusion Coating Grade
Dow LDPE 5004I Low Density Polyethylene, Extrusion Coating Grade

PCARM009 / 79747

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.