MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Copper Alloy, UNS C69350, M10 Temper, Castings
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Temper: As Hot Forged - Air Cooled

Fabrication Properties: Excellent Suitability – Soldering, Capacity for Being Hot Formed; Good Suitability – Brazing, Oxyacetylene Welding, Gas Shielded Arc Welding, Coated Metal Arc Welding, Spot Weld, Seam Weld, Butt Weld; Poor Suitability – Capacity for Being Cold Worked

Typical uses: Marine Components; Potable water system components; Valve Bodies, Faucets and Plumbing Components

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.297 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 120
@Load 3000 kg
Tensile Strength 71.1 ksiTypical
 66.7 - 78.3 ksi
Elongation at Break 15 - 25 %
Machinability 75 %
Forgeability 95 %
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000260 ohm-cm6.5% IACS
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.54 µin/in-°F
@Temperature 20.0 - 100 °C
 10.83 µin/in-°F
@Temperature 20.0 - 200 °C
 11.5 µin/in-°F
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.0950 BTU/lb-°F
Thermal Conductivity 20.13 BTU-in/hr-ft²-°F
Melting Point >= 1546 °F
Solidus 1546 °F
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al <= 0.10 %
Copper, Cu 73 - 77 %
Iron, Fe 0.10 - 0.50 %
Lead, Pb <= 0.20 %
Manganese, Mn <= 0.10 %
Nickel, Ni <= 0.10 %
Phosphorus, P 0.040 - 0.10 %
Silicon, Si 3.0 - 3.4 %
Tin, Sn <= 0.20 %
Zinc, Zn 18.8 - 23.9 %As Balance

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

MC69350x2 / 292381

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.