MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Advanced Elastomer Systems VistaFlex® 715-B Thermoplastic Rubber  (discontinued **)
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Elastomer, Melt-Processible Rubber

Material Notes: Description: A black high-flow thermoplastic elastomer especially designed for injection molding applications. It replaces soft thermoplastics such as SBS, SEBS, and PVC blends. Supplied as free-flowing pellets in 25 kilogram (55 pound) moisture barrier bags.

Features:

  • High flow
  • Good surface appearance on molded parts
  • Good tensile properties and high elongation at break
  • Good tear strength

Product Notes: Values are for injection molded plaques, side gated.
82.6 mm x 117.5 mm x 3 mm

Information provided by Advanced Elastomer Systems.

Advanced Elastomer Systems is now a part of ExxonMobil. This grade was removed from the Advanced Elastomers Systems standard product line before the ExxonMobil acquisiton.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.05 g/ccASTM D792
Melt Flow 35 g/10 min
@Load 5.00 kg,
Temperature 230 °C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 855 seconds; ASTM D2240
Tensile Strength at Break 649.6 psiAfter 3000 hrs. Xenon test 1200; ISO 4665
 928 psiAcross flow; ASTM D412
Tensile Strength, Yield 595 psiAt 100% elongation, across flow; ASTM D412
Elongation at Break 525 %After 3000 hrs. Xenon test 1200; ISO 4665
 700 %Across flow; ASTM D412
Tensile Modulus 0.110 GPa1mm/min; DIN 53457
Flexural Modulus 0.105 GPa1.7 mm/min; DIN 53457
Izod Impact, Notched NB
@Temperature -30.0 °C
ISO 180A
Tear Strength 280 pli73°F; ASTM D624
Compression Set 38 %
@Temperature 22.8 °C,
Time 79200 sec
Method B; ASTM D395
 55 %
@Temperature 70.0 °C,
Time 79200 sec
Method B; ASTM D395
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 53.0 °CVicat A, 1 kg; DIN 53460/ISO 306
Brittleness Temperature -58.0 °FASTM D746
 
Processing PropertiesOriginal ValueComments
Processing Temperature 175 - 240 °C
Mold Temperature 20.0 - 40.0 °C

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Solvay Engineered Polymers Dexflex® 756-67 TPO
Advanced Elastomer Systems VistaFlex® 641N Thermoplastic Rubber
Advanced Elastomer Systems Vistaflex® 671N Thermoplastic Rubber
Advanced Elastomer Systems VistaFlex® 714-B Thermoplastic Rubber
Advanced Elastomer Systems VistaFlex® 714-N Thermoplastic Rubber

PADW612 / 22900

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.