MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Envalior Stanyl® TW200B6 PA46-CF30
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 46 (PA46)

Material Notes: 30% Carbon Reinforced, Heat Stabilized, Lubricated

Former DSM Engineering Plastics product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.28 g/ccdry; ISO 1183
Moisture Absorption 2.60 %Sim. To ISO 62
Linear Mold Shrinkage, Flow 0.0020 cm/cmISO 294-4
Linear Mold Shrinkage, Transverse 0.0090 cm/cmISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 150 MPacond; ISO 527-1/-2
 240 MPadry; ISO 527-1/-2
 95.0 MPa
@Temperature 180 °C
ISO 527-1/-2
 105 MPa
@Temperature 160 °C
ISO 527-1/-2
 125 MPa
@Temperature 120 °C
ISO 527-1/-2
Elongation at Break 2.0 %dry; ISO 527-1/-2
 4.0 %cond; ISO 527-1/-2
 3.0 %
@Temperature 120 °C
ISO 527-1/-2
 3.0 %
@Temperature 160 °C
ISO 527-1/-2
 3.0 %
@Temperature 180 °C
ISO 527-1/-2
Tensile Modulus 24.0 GPadry; ISO 527-1/-2
 8.30 GPa
@Temperature 180 °C
ISO 527-1/-2
 8.80 GPa
@Temperature 160 °C
ISO 527-1/-2
 10.0 GPa
@Temperature 120 °C
ISO 527-1/-2
Flexural Modulus 9200 MPacond; ISO 178
 18500 MPadry; ISO 178
Fatigue Strength 60.0 MPa
@# of Cycles 1.00e+7 ,
Temperature 140 °C
R = 0.1, 8 Hz, dry
 67.0 MPa
@# of Cycles 1.00e+6 ,
Temperature 140 °C
R = 0.1, 8 Hz, dry
 77.0 MPa
@# of Cycles 100000 ,
Temperature 140 °C
R = 0.1, 8 Hz, dry
 87.0 MPa
@# of Cycles 10000 ,
Temperature 140 °C
R = 0.1, 8 Hz, dry
 100 MPa
@# of Cycles 1000 ,
Temperature 140 °C
R = 0.1, 8 Hz, dry
 115 MPa
@# of Cycles 100 ,
Temperature 140 °C
R = 0.1, 8 Hz, dry
Izod Impact Resistance 0.650 J/cm²
@Temperature -40.0 °C
cond; ISO 180/1A
 0.650 J/cm²
@Temperature -40.0 °C
dry; ISO 180/1A
 0.800 J/cm²
@Temperature 23.0 °C
dry; ISO 180/1A
 1.40 J/cm²
@Temperature 23.0 °C
cond; ISO 180/1A
Charpy Impact Unnotched 50.0 kJ/m²
@Temperature -30.0 °C
cond; ISO 179/1eU
 50.0 kJ/m²
@Temperature -30.0 °C
dry; ISO 179/1eU
 60.0 kJ/m²
@Temperature 23.0 °C
dry; ISO 179/1eU
 75.0 kJ/m²
@Temperature 23.0 °C
cond; ISO 179/1eU
Charpy Impact, Notched 6.50 kJ/m²
@Temperature -30.0 °C
cond; ISO 179/1eA
 6.50 kJ/m²
@Temperature -30.0 °C
dry; ISO 179/1eA
 8.00 kJ/m²
@Temperature 23.0 °C
dry; ISO 179/1eA
 14.0 kJ/m²
@Temperature 23.0 °C
cond; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 100 ohm-cmdry; IEC 60093
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 8.00 µm/m-°Cdry; ISO 11359-1/-2
CTE, linear, Transverse to Flow 34.0 µm/m-°Cdry; ISO 11359-1/-2
Melting Point 295 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 290 °Cdry; ISO 75-1/-2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Envalior Stanyl® TW241B3 PA46-CF15
Envalior Stanyl® TW200B6 PA46-CF30, Conditioned, 30% Carbon Reinforced, Heat Stabilized
Envalior Stanyl® TS200F6 PA46-GF30
Envalior Stanyl® TW200B6 PA46-CF30, Dry, 30% Carbon Reinforced, Heat Stabilized
Envalior Stanyl® TS241B3 PA46-CF15

PDSM9900 / 161521

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.