MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Magnesium AZ91E-T6, Cast
Categories: Metal; Nonferrous Metal; Magnesium Alloy

Material Notes: Magnesium AZ91A, B, C, D, and E have the same nominal composition but differ in ranges and/or specified impurity limits. This high purity alloy has excellent corrosion resistance. Commonly used in pressure-tight sand and permanent mold castings with high tensile strength and moderate yield strength. General purpose alloy, high strength.

Key Words: UNS M11919; Mg; European EN 1753 MC 21120; AMS 4446; ASTM B 94;SAE J465 (Ingot UNS M11918)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.81 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 70500 kg load, 10 mm ball
Hardness, Knoop 93Estimated from Brinell
Hardness, Rockwell E 77
Hardness, Vickers 80Estimated from Brinell
Tensile Strength, Ultimate 275 MPa
Tensile Strength, Yield 145 MPa
@Strain 0.2 %
Elongation at Break 6.0 %in 50 mm
Tensile Modulus 44.8 GPa
Compressive Yield Strength 130 MPaat 0.2% offset
Ultimate Bearing Strength 515 MPa
Bearing Yield Strength 360 MPa
Poissons Ratio 0.35
Fatigue Strength 85.0 MPa
@# of Cycles 5.00e+8
R.R. Moore Test
Shear Modulus 17.0 GPa
Charpy Impact 1.40 JV-Notch
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000129 ohm-cm(AZ91C-T6)
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 373 J/g
CTE, linear 26.0 µm/m-°C
@Temperature 25.0 °C
 27.2 µm/m-°C
@Temperature 20.0 - 200 °C
Specific Heat Capacity 1.047 J/g-°C
Thermal Conductivity 72.7 W/m-K
Melting Point >= 421 °CIncipient Melting
Solidus 470 °C
Liquidus 595 °C
 
Processing PropertiesOriginal ValueComments
Casting Temperature 650 - 815 °CPermanent Mold Casting
 705 - 845 °CSand Casting
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 8.1 - 9.3 %
Copper, Cu <= 0.015 %
Iron, Fe <= 0.0050 %
Magnesium, Mg 88.51 - 91.22 %As Remainder
Manganese, Mn 0.17 - 0.35 %
Nickel, Ni <= 0.0010 %
Other, total <= 0.30 %
Silicon, Si <= 0.20 %
Zinc, Zn 0.40 - 1.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Magnesium AZ91E-T4, Cast
Magnesium AZ91E-F, Cast
Magnesium AZ91D-F, Cast
Magnesium AZ91C-T6, Cast
Magnesium AZ91A-F, Die Cast

MMAZ93 / 12339

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.