MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

NOVA Chemicals SURPASS® RMs245-U sHDPE Rotational Molding Resin
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Rotational Molding Grade

Material Notes:

Octene Copolymer

Features:

  • Exceptional low temperature impact properties
  • Broad processing window
  • High stiffness for very large tanks, combined with exceptional ESCR performance
  • Superior whiteness for improved part appearance, resistant to gas fading
  • NSF listed for Standards #24, 51, 61
  • Broad application use and potential for resin consolidation
  • Good interior finish on large tanks
  • UL94 HB
  • HDB rating 1600 psi

Additives:

  • Processing antioxidants
  • UV stabilizers (estimated UV resistance > UV20)

Applications:

  • Septic tanks
  • Very large tanks (up to 20,000 gallons)
  • Agricultural tanks as small as 3,000 gallons

United States: SURPASS RMs245-U(UG) resin complies with the specifications contained in the U.S. Food and Drug Administration (FDA) regulation 21 CFR 177.1520 for olefin polymers, para. (c) 3.2a, and may thus be used in the United States as an article or component of an article intended for use in contact with food. This resin is subject to the specific limitation that it may contact food only at temperatures of 212°F and below (21 CFR 176.170(c) Table 2, conditions of use B–H).

NOVA Chemicals polyethylene resins are biologically and chemically inert.

Information provided by NOVA Chemicals®

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.945 g/cc0.0341 lb/in³ASTM D 792
ESCR 100% Igepal® >= 1000 hour
@Temperature 50.0 °C
>= 1000 hour
@Temperature 122 °F
F50, Condition A & B; ASTM D 1693
Melt Index of Compound 1.7 g/10 min
@Load 2.16 kg,
Temperature 190 °C
1.7 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D 1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 23.0 MPa
@Thickness 1.91 mm
3340 psi
@Thickness 0.0750 in
Type IV specimen, 2" (50.8 mm) per minute test speed; ASTM D 638
Elongation at Yield 11 %
@Thickness 1.91 mm
11 %
@Thickness 0.0750 in
Type IV Specimen, 2" (50.8 mm) per minute test speed; ASTM D 638
Flexural Modulus 1.03 GPa
@Strain 1 %
149 ksi
@Strain 1 %
ASTM D 790
Impact Test  75.0 J
@Thickness 3.17 mm,
Temperature -40.0 °C
55.3 ft-lb
@Thickness 0.125 in,
Temperature -40.0 °F
ARM Low Temperature Impact; ARM Method
 >= 245 J
@Thickness 6.35 mm,
Temperature -40.0 °C
>= 181 ft-lb
@Thickness 0.250 in,
Temperature -40.0 °F
ARM Low Temperature Impact; ARM Method
 
Thermal PropertiesMetricEnglishComments
Melting Point 127 °C261 °F(DSC)
Heat Distortion Temperature  43.0 °C
@Pressure 1.82 MPa
109 °F
@Pressure 264 psi
ASTM D 648
 63.0 °C
@Pressure 0.455 MPa
145 °F
@Pressure 66.0 psi
ASTM D 648
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
NOVA Chemicals SURPASS® RMs245-UG sHDPE Rotational Molding Resin
ICO Polymers ICORENE™ 150-1049 HDPE Rotational Molding Resin
ICO Polymers ICORENE™ 150-1498 HDPE Rotational Molding Resin
A. Schulman POLYAXIS® LP624 Stabilized High Density Polyethylene
ICO Polymers ICORENE™ 150-1497 HDPE Rotational Molding Resin

PNOVB095 / 194703

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.