MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Elastron® Elastron® G F.G100.A55.N SEBS
Categories: Polymer; Thermoplastic; Styrene-Butadiene

Material Notes: Product Description: A soft, colorable SEBS based thermoplastic elastomer (TPE) compound designed for contact with non-fatty foods. The monomers and additives used to produce this product are listed in the Union List of Authorized Substances of Regulation 10/20/11/EC. Bondable to: PP, EVA, PE
Availability: Africa & Middle East; Asia Pacific; Europe; North America
Features: Block Copolymer; Bondability; Food Contact Acceptable; Good Colorability; Soft
Agency Ratings: EU 2011/10/EC
RoHS Compliance: RoHS Compliant
Appearance: Natural Color
Forms: Pellets
Processing Method: Injection Molding

Information provided by Elastron

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.17 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.019 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.0091 in/inASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 55ASTM D2240
Tensile Strength at Break 580 psiASTM D412
Tensile Stress 218 psi
@Strain 100 %
ASTM D412
 305 psi
@Strain 300 %
ASTM D412
Elongation at Break 700 %ASTM D412
Tear Strength 154 pliASTM D624
Compression Set 19 %
@Temperature 22.8 °C,
Time 79200 sec
ASTM D395
 45 %
@Temperature 70.0 °C,
Time 79200 sec
ASTM D395
 67 %
@Temperature 100 °C,
Time 79200 sec
ASTM D395
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 293 - 347 °F
Middle Barrel Temperature 311 - 365 °F
Front Barrel Temperature 320 - 374 °F
Nozzle Temperature 347 - 401 °F
Mold Temperature 77.0 - 122 °F
 
Descriptive Properties
Ozone ResistanceNo CracksStressed, ASTM D518
Suggested Max Regrind0.2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PELAST180 / 267762

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.