MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Dow Bynel® 30E753 Anhydride Modified Ethylene Vinyl Acetate
Categories: Polymer; Thermoplastic; Ethylene Vinyl Acetate; Ethylene Vinyl Acetate Copolymer (EVA), Adhesive/Sealant Grade

Material Notes: BYNEL® Series 3000 resins are anhydride-modified ethylene vinyl acetate polymers. They are available in pellet form for use in conventional extrusion and coextrusion equipment designed to process polyethylene (PE) resins.

Physical properties of BYNEL Series 3000 resins are typical of EVA resins with similar density and melt index values.

BYNEL 30E753 is specifically designed to provide high adhesion to both metals and polyolefins when converted into film form and used as a thermal lamination film. It has a low coefficient of friction for easy film handling and provides strong bonds that fail cohesively. BYNEL 3000 series resins adhere to a wide variety of materials. They are most often used to adhere to PE, ionomers, EVA and polyamide.

BYNEL 30E753 resin conforms with the Code of Federal Regulations, Title 21, Paragraph 175.105, covering the use of adhesive interlayers in composite packages for food use. This regulation describes adhesives which may be safely used as components of articles intended for use in packaging, transporting or holding food. This regulation requires that either (1) the adhesive is separated from the food by a functional barrier, or (2) the quantity of adhesive which contacts fatty or aqueous foods does not exceed the trace amounts at the seams or edges. Customers should satisfy themselves that the food contact material is serving as a functional barrier to the adhesive.

This former DuPont product line is now a Dow product line.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.938 g/ccASTM D792, ISO 1183
Melt Flow 2.1 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238, ISO 1133
 
Thermal PropertiesOriginal ValueComments
Melting Point 89.0 °CFreezing Point; ASTM D3418
 92.0 °CASTM D3418, ISO 3146
Vicat Softening Point 65.0 °CASTM D1525, ISO 306
 
Processing PropertiesOriginal ValueComments
Processing Temperature <= 235 °C
Feed Temperature 135 °CBlown Film Coextrusion
Zone 2 160 °CBlown Film Coextrusion
Zone 3 185 °CBlown Film Coextrusion
Zone 4 185 °CBlown Film Coextrusion
Zone 5 185 °CBlown Film Coextrusion
Adapter Temperature 185 °CBlown Film Coextrusion
Die Temperature 185 °CBlown Film Coextrusion
Melt Temperature <= 235 °CCoExtrusion with EVA Processing

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Dow Bynel® 30E783 Anhydride Modified Ethylene Vinyl Acetate
Dymax 3073 Solvent-Free Plastic Adhesive
Covestro Bayhydrol® A 145 Polyurethane Coating
ExxonMobil LD 145.PX Packaging Resin
LyondellBasell Plexar® PX5125 Extrudable Tie-Layer Resin - Anhydride Modified LLDPE

PDTA4920 / 170360

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.