MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Ascend Performance Materials Starflam® RF0069 PA66, 30% Glass Fiber, Flame Retardant, Injection Molded
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled; Nylon 66, Glass Fiber Filled, Flame Retardant

Material Notes: Starflam RF0069 is a Flame Retardant, 30% Glass Reinforced Polyamide 66 Injection Molding Resin (also known as PA66 30V U2 Z79 or RF1006Z590)

Former Eurostar product. Eurostar has been acquired by Ascend Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.58 g/ccDAM; ISO 1183
Water Absorption at Saturation 4.0 %ISO 62
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 165 MPaDAM; ISO 527-2
Elongation at Break 2.0 %DAM; ISO 527-2
Tensile Modulus 9500 MPaDAM; ISO 527-2
Flexural Strength 190 MPaDAM; ISO 178
Flexural Modulus 9300 MPaDAM; ISO 178
Izod Impact, Notched (ISO) 7.00 kJ/m²
@Temperature -30.0 °C
DAM; ISO 180/1A
 8.00 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
Charpy Impact Unnotched 60.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eU
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index 250 V
@Thickness 3.00 mm
IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 23.0 µm/m-°C
@Thickness 2.00 mm,
Temperature 35.0 - 55.0 °C
DAM; ISO 11359-2
CTE, linear, Transverse to Flow 72.0 µm/m-°C
@Thickness 2.00 mm,
Temperature 23.0 - 55.0 °C
DAM; ISO 11359-2
UL RTI, Electrical 65.0 °C
@Thickness 0.750 mm
UL 746
 65.0 °C
@Thickness 3.00 mm
UL 746
UL RTI, Mechanical with Impact 65.0 °C
@Thickness 0.750 mm
UL 746
 65.0 °C
@Thickness 3.00 mm
UL 746
UL RTI, Mechanical without Impact 65.0 °C
@Thickness 0.750 mm
UL 746
 65.0 °C
@Thickness 3.00 mm
UL 746
Flammability, UL94 V-0
@Thickness 0.750 mm
 V-0
@Thickness 3.00 mm
Oxygen Index 31 %DAM; EN ISO 4589-2
Glow Wire Flammability Index 960 °C
@Thickness 2.00 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 270 - 290 °CInjection
Middle Barrel Temperature 270 - 280 °CInjection
Front Barrel Temperature 270 - 280 °CInjection
Melt Temperature 270 - 280 °CInjection
Mold Temperature 70.0 - 100 °CInjection
Drying Temperature 75.0 - 85.0 °CInjection
Dry Time 4.00 hourInjection
Moisture Content 0.20 %Injection
 
Descriptive Properties
AdditiveFlame Retarding Agent
 Heat Stabilizer
 Release agent
AppearanceNatural Color
FeaturesFlame Retardant
 Halogenated
FormsPellets
Processing MethodInjection Molding
RegionNorth America, Europe
UL File NumberE70062

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Grupo Repol Dinalon® A1S25 G30 PA66 30% Glass Fiber
PTS Trimid® N66-G33 33% Glass Fiber Reinforced Nylon 6/6
PTS Trimid® N66-G33L 33% Glass Fiber Reinforced Lubed Nylon 6/6
Envalior Durethan® AKV 30 H2.0 901510 Nylon 66 (PA66), 30% Glass Fiber Reinforced, Conditioned
Envalior Durethan® AKV 30 GIT H2.0 900116 Nylon 66 (PA66), 30% Glass Fiber Reinforced, Dry

PEUROSTA49 / 172063

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.