MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Eastman Eastar AN001 Copolyester, Natural
Categories: Polymer; Thermoplastic; Polyester, TP

Material Notes: Eastar AN001 Copolyester has excellent appearance and is nearly water-clear. Its most outstanding features are its chemical resistance and processing capabilities. Exposure to aromatic oils often causes crazing or actual fracture of many polymer resins, but AN001 maintains its physical properties when exposed to these oils, and its appearance is virtually unchanged.

Applications/Uses

  • Cosmetics/personal care packaging
  • Fragrance packaging
  • Key Attributes

  • Effective barrier properties
  • Excellent Clarity
  • Excellent colorability
  • Good stiffness
  • Excellent chemical resistance
  • Toughness
  • Easy to extrude, cut, print, and seal
  • High gloss appearance
  • Good impact strength

  • Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Specific Gravity 1.20 g/cc1.20 g/ccASTM D792
    Linear Mold Shrinkage 0.0020 - 0.0060 cm/cm
    @Thickness 3.20 mm
    0.0020 - 0.0060 in/in
    @Thickness 0.126 in
    ASTM D955
     
    Mechanical PropertiesMetricEnglishComments
    Hardness, Rockwell R 103103ASTM D785
    Tensile Strength at Break 51.0 MPa7400 psiASTM D638
    Tensile Strength, Yield 47.0 MPa6820 psiASTM D638
    Elongation at Break 320 %320 %ASTM D638
    Elongation at Yield 5.0 %5.0 %ASTM D638
    Flexural Yield Strength 69.0 MPa10000 psiASTM D790
    Flexural Modulus 2.00 GPa290 ksiASTM D790
    Izod Impact, Notched  0.400 J/cm
    @Temperature -40.0 °C
    0.749 ft-lb/in
    @Temperature -40.0 °F
    ASTM D256
     0.800 J/cm
    @Temperature 23.0 °C
    1.50 ft-lb/in
    @Temperature 73.4 °F
    ASTM D256
    Izod Impact, Unnotched NBNBASTM D4812
     NB
    @Temperature -40.0 °C
    NB
    @Temperature -40.0 °F
    ASTM D4812
    Puncture Energy 42.0 J31.0 ft-lbPuncture Resistance @Max Load, 23°C; ASTM D3763
     48.0 J
    @Temperature -40.0 °C
    35.4 ft-lb
    @Temperature -40.0 °F
    Puncture Resistance at Max Load; ASTM D3763
     
    Thermal PropertiesMetricEnglishComments
    Deflection Temperature at 0.46 MPa (66 psi) 73.0 °C163 °FASTM D648
    Deflection Temperature at 1.8 MPa (264 psi) 65.0 °C149 °FASTM D648
     
    Optical PropertiesMetricEnglishComments
    Haze 0.30 %0.30 %ASTM D1003
    Transmission, Visible 89 %89 %Regular Transmittance; ASTM D1003
     91 %91 %Total Transmittance; ASTM D1003
     
    Processing PropertiesMetricEnglishComments
    Melt Temperature 230 - 280 °C446 - 536 °F
    Mold Temperature 15.0 - 30.0 °C59.0 - 86.0 °F
    Drying Temperature 70.0 °C158 °F
    Dry Time 3 hour3 hour

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    Eastman DuraStar DS1000 Polymer, Natural
    Eastman Eastar EN067 Copolyester, Natural
    Eastman DURASTAR DS1010 Natural PCTA Copolyester
    Eastman DuraStar DS1900HF Polymer, Natural
    Eastman Eastalloy DA003 PC+PCTG Copolyester/Polycarbonate

    PE9023 / 35079

    Aluminum Castings

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.