MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
INEOS Styrolution Polystyrol 168 N GR 21 PS
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene, Molded, Unreinforced

Material Notes: Description: Polystyrol 168 N is a high molecular, heat grade used where high strength is required. Suitable for physically or chemically expanded extruded sheet. As blend component with high impact Polystyrol or Styrolux.

Applications: Foamed meat trays, foamed labels. In mixture with high impact Polystyrene for coffee cups, lids. In mixture with Styrolux for transparent, impact resistant cups, breakers and lids.

Information provided by STYROLUTION, which is a joint venture between BASF and INEOS

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.048 g/ccISO 1183
Water Absorption <= 0.10 %ISO 62
Moisture Absorption at Equilibrium <= 0.10 %23°C/50% RH; ISO 62
Melt Flow 1.572 g/10 min
@Load 5.00 kg,
Temperature 200 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 150 MPa
@Load 36.5 kg,
Time 30.0 sec
ISO 2039-1
Tensile Strength at Break 59.0 MPaISO 527-1/-2
Elongation at Break 3.0 %ISO 527-1/-2
Tensile Modulus 3300 MPaISO 527-1/-2
Flexural Strength 106 MPaISO 178
Flexural Modulus 2300 MPaASTM D790
Shear Modulus 1.45 GPaISO 6721-2
Charpy Impact Unnotched <= 25.0 kJ/m²ISO 179/1eU
Charpy Impact, Notched 4.00 kJ/m²ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+16 ohm-cmIEC 60093
Surface Resistance >= 1.00e+14 ohmIEC 60093
Dielectric Constant 2.5
@Frequency 1e+6 Hz
IEC 60250
 2.5
@Frequency 100 Hz
IEC 60250
Dielectric Strength 135 kV/mmK20/P50; IEC 60243-1
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 98.0 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 86.0 °CISO 75-1/-2
Vicat Softening Point 101 °CVST/B/50; ISO 306
 108 °CVST/A/120; ISO 306
Flammability, UL94 HB
@Diameter 1.60 mm
IEC 60695-11-10
 HB
@Diameter 3.18 mm
IEC 60695-11-10
 
Optical PropertiesOriginal ValueComments
Transmission, Visible 90 %transparent; thickness not quantified
 
Processing PropertiesOriginal ValueComments
Melt Temperature 210 - 240 °CFlat film
 180 - 280 °CInjection Molding
Mold Temperature 10.0 - 60.0 °CInjection Molding
 
Descriptive Properties
ColorCrystal Clear 00013
Commercial StatusEurope
Primary Processing TechniqueInjection Molding and Extrusion

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chi Mei Polyrex® PH-88 Polystyrene - High Impact
Bamberger Polymers Bapolan® 6045 Polystyrene, Injection Grade
INEOS Styrolution Polystyrol 168 N GR 2 PS
Americas Styrenics STYRON™ 668 General Purpose Polystyrene Resin
INEOS Styrolution Polystyrol 158 K GR 21 PS

PBASG0628 / 132261

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.