MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Murtfeldt Murylon® B Nylon 6
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Impact Grade

Material Notes: Murylon® B natural has the best impact resistance of all Murylon materials. This material is especially suited for use in machine construction thanks to an excellent combination of mechanical properties.

Special Properties:
• Exceptional resistance
• Good impact strength
• Low cold flow characteristics
• Approved for use in the food industry (EU and FDA

Information provided by Murtfeldt Kunststoffe GmbH & Co. KG.

Key Words: PA 6
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.14 g/ccISO 1183-1
Moisture Absorption at Equilibrium 2.6 %
@Temperature 23.0 °C
50% RH
Water Absorption at Saturation 9.0 %
@Temperature 23.0 °C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 85dry; ISO 2039-2
Hardness, Shore D 76DIN 53505
Ball Indentation Hardness 150 MPadry; ISO 2039-1
Tensile Strength, Yield 45.0 MPa50% RH; ISO 527-1
 80.0 MPadry; ISO 527-1
Elongation at Break >= 50 %dry; ISO 527-1
 >= 100 %50% RH; ISO 527-1
Creep Strength 7.00 MPa
@Time 3.60e+6 sec
stress leading to 1% elongation; 50% RH; ISO 899-1
 18.0 MPa
@Time 3.60e+6 sec
stress leading to 1% elongation; dry; ISO 899-1
Modulus of Elasticity 1.425 GPa50% RH
 3.30 GPadry
Compressive Yield Strength 24.0 MPa
@Strain 1 %
dry; ISO 604
 46.0 MPa
@Strain 2 %
dry; ISO 604
 80.0 MPa
@Strain 5.0 %
dry; ISO 604
Charpy Impact Unnotched NBdry; ISO 179-1/1eU
 NBISO 179
Charpy Impact, Notched 5.50 kJ/m²dry; ISO 179-1/1eA
Coefficient of Friction, Dynamic 0.35
Sand Slurry 0.23µm/km
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity >= 1.00e+12 ohm-cm50% RH; IEC 60093
 >= 1.00e+14 ohm-cmdry; IEC 60093
Surface Resistance >= 1.00e+12 ohm50% RH; IEC 60093
 >= 1.00e+13 ohmdry; IEC 60093
Dielectric Constant 3.3
@Frequency 1e+6 Hz
dry; IEC 60250
 3.8
@Frequency 1e+6 Hz
50% RH; IEC 60250
 3.9
@Frequency 100 Hz
dry; IEC 60250
 7.4
@Frequency 100 Hz
50% RH; IEC 60250
Dielectric Strength 16.0 kV/mm50% RH; IEC 60243-1
 25.0 kV/mmdry; IEC 60243-1
Dielectric Loss Index 0.019
@Frequency 100 Hz
dry; IEC 60250
 0.021
@Frequency 1e+6 Hz
dry; IEC 60250
 0.060
@Frequency 1e+6 Hz
50% RH; IEC 60250
 0.13
@Frequency 100 Hz
50% RH; IEC 60250
 
Thermal PropertiesOriginal ValueComments
CTE, linear 90.0 µm/m-°C
@Temperature 23.0 - 60.0 °C
 105 µm/m-°C
@Temperature 23.0 - 100 °C
Thermal Conductivity 0.280 W/m-K
Melting Point 220 °CISO 11357-1
Maximum Service Temperature, Air 70.0 °C
@Time 7.20e+7 sec
 85.0 °C
@Time 1.80e+7 sec
 160 °C
@Time <=86400 sec
Minimum Service Temperature, Air -40.0 °C
Glass Transition Temp, Tg 50.0 °CISO 11357-1
Flammability, UL94 HB
 
Compliance PropertiesOriginal ValueComments
European Food 1935/2004 Yes
FDA Yes
 
Descriptive Properties
ColorNatural/Black

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Arkema Pebax® 7233 SP 01 TPA
Isoflon PVC Polyvinyl Chloride
GEHR Plastics PVC type II®
Röchling SUSTAMID® 6 FR PA 6
Röchling SUSTAGLIDE® PA 6

PMURT921 / 156568

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.