MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Meldin Supplier

(Viewing data as-entered. Click here to return)
Saint-Gobain Meldin® 2211 Bearing
Categories: Polymer; Thermoset; Polyimide, TS

Material Notes: General Notes on Meldin 2000 Series Bearing Products:
For High-Temperature, Close-Tolerance Applications. Able to withstand temperatures of 600°F with excursions to 900°F, the Medlin® 2000 Series can be machined into various configurations, from rod or sheet stock shapes. Black in color. Meldin® 2000 Series offers very high compression strength, high creep resistance, and dimensional stability.
Specific Notes on Meldin® 2211 Bearing
Meldin® 2211 offers the balanced properties of low friction, high strength and resistance to compressive creep.

Applications include: Appliances, Automotive, Industrial, Semiconductor, Transportation.

Specification Notes: Note that the specifications given for this product are typical specifications for the Meldin® 2000 Series, and individual products will vary as indicated in the material notes.
Information provided by Saint Gobain Performance Products.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.53 g/ccASTM D792
Water Absorption 0.18 %ASTM D570
Deformation 0.10 %
@Pressure 13.8 MPa
24 hrs. Mold Direction; ASTM D621
Outgassing - Total Mass Loss 0.50 %% WVR; ASTM E595
 1.19 %ASTM E5955
Collected Volatile Condensable Material 0.010 %ASTM E55955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 85ASTM D2240
Tensile Strength, Ultimate 22.0 MPa
@Temperature 260 °C
ASTM D 638
 46.8 MPa
@Temperature 23.0 °C
ASTM D 638
Elongation at Break 3.0 %
@Temperature 260 °C
ASTM D 638
 4.0 %
@Temperature 23.0 °C
ASTM D 638
Tensile Modulus 0.700 GPa
@Temperature 260 °C
ASTM D 638
 2.00 GPa
@Temperature 23.0 °C
ASTM D 638
Flexural Strength 79.2 MPaASTM D 790
Flexural Modulus 3.80 GPaASTM D 790
Izod Impact, Notched 19.8 J/mASTM D 256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmASTM D257
Surface Resistance 1.00e+15 ohmASTM D257
Dielectric Constant 5.47
@Frequency 1e+6 Hz
ASTM D150
 5.53
@Frequency 10000 Hz
ASTM D150
 5.56
@Frequency 100 Hz
ASTM D150
Dissipation Factor 0.0019
@Frequency 100 Hz
ASTM D150
 0.0028
@Frequency 10000 Hz
ASTM D150
 0.0035
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesOriginal ValueComments
CTE, linear 58.0 µm/m-°CASTM E831-93
Thermal Conductivity 0.400 W/m-KC518/C177
Maximum Service Temperature, Air >= 600 °FUL-746 B

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSTGQZ103 / 68614

Ensinger SPI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.