MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

PlastiComp Complet® LCF30 - PA6 Nylon 6, 30% Long Carbon Fiber Reinforced  (discontinued **)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Carbon Fiber Filled

Material Notes: Complet® long-fiber reinforced pellets are manufactured to exceed expectation for quality and performance.

Nylon 6 with 30% carbon fiber reinforcement

Information provided by PlastiComp, Inc.

Key Words: Complet® Long Fiber LCF
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.27 g/cc1.27 g/ccASTM D-792
Filler Content 30 %30 %Carbon Fiber
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 269 MPa39000 psiASTM D-638
Elongation at Break 1.0 - 2.0 %1.0 - 2.0 %ASTM D-638
Tensile Modulus 22.069 GPa3200.8 ksiASTM D-638
Flexural Strength 379 MPa55000 psiASTM D-790
Flexural Modulus 16.207 GPa2350.6 ksiASTM D-790
Izod Impact, Notched 2.14 J/cm4.01 ft-lb/inASTM D-256
Izod Impact, Unnotched 9.08 J/cm17.0 ft-lb/inASTM D-4812
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 260 - 277 °C500 - 530 °F
Middle Barrel Temperature 266 - 282 °C510 - 540 °F
Front Barrel Temperature 271 - 288 °C520 - 550 °F
Nozzle Temperature 271 - 288 °C520 - 550 °F
Melt Temperature 271 - 288 °C520 - 550 °F
Mold Temperature 93.3 °C200 °F
Injection Velocity 50.8 - 76.2 mm/sec2.00 - 3.00 in/sec
Drying Temperature 85.0 °C
@Time 14400 sec
185 °F
@Time 4.00 hour
Moisture Content <= 0.18 %<= 0.18 %
Back Pressure 0.172 - 0.345 MPa25.0 - 50.0 psi
Cushion 0.635 cm0.250 in
Screw Speed 30 - 50 rpm30 - 50 rpm
 
Descriptive Properties
Injection PressureMedium to maximum

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Nanocyl PLASTICYL™ PA1503 Polyamide 6 with 3 wt% of Multi-Wall Carbon Nanotubes
PlastiComp Complet® LCF30-PA66 30% Long Carbon Fiber
PlastiComp Complet® LCF40 - PA6 Nylon 6, 40% Long Carbon Fiber Reinforced
Aluminum 380.0-F Die Casting Alloy
Aluminum 360.0-F Die Casting Alloy

PPLASTI925 / 159578

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.