MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Solvay APC-2-PEEK Unreinforced
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK)

Material Notes: Cytec Engineered Materials APC-2 composites have a thermoplastic matrix of poly(ether-ether-ketone) commonly referred to as PEEK. The polymer is semi-crystalline with a glass transition temperature of 289°F (143°C). Composites can be used in lightly loaded applications at temperatures up to 500°F (260°C) due to the semi-crystalline nature of the polymer. The composites possess excellent environmental resistance, toughness and fire resistant properties. APC-2 prepreg can be stored at ambient conditions and has an indefinite shelf life. APC02 composites retain good mechanical properties at cryogenic temperatures. The excellent composite properties result from the PEEK matrix, the full wetting and tailored fiber matrix interface achieved in the impregnation process. Laminates and parts can be fabricated from APC-2 using a wide range of processes from autoclave consolidation to rapid stamping techniques. The prepreg may also be filament wound and tape-placed using in-situ consolidation. This wide range of processing techniques may be used because of the thermoplastic nature of the polymer and the full wetting of the fibers in the prepreg.

Features & Benefits:

  • Fully impregnated, unidirectional prepreg
  • Large database
  • Very high toughness and damage tolerance
  • Good resistance to creep and fatigue
  • Very good wear resistance
  • Processed using a wide range of fabrication techniques at 720°F (382°C)
Applications: Typical applications for Cytec Engineered Materials APC-2 include aircraft structure, space components and other structural engineering components

Data for unreinforced PEEK; separate entries report composite property data.

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.32 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 8500 psi
@Temperature 121 °C
 8500 psi
@Temperature 121 °C
Wet
 14500 psi
@Temperature 24.0 °C
Elongation at Break 70 %
@Temperature 24.0 °C
 70 %
@Temperature 121 °C
 70 %
@Temperature 121 °C
Wet
Tensile Modulus 3.40 GPa
@Temperature 121 °C
 3.40 GPa
@Temperature 121 °C
Wet
 3.60 GPa
@Temperature 24.0 °C
Flexural Strength 14500 psi
@Temperature 121 °C
 14500 psi
@Temperature 121 °C
Wet
 24700 psi
@Temperature 24.0 °C
Flexural Modulus 4.00 GPa
@Temperature 121 °C
 4.00 GPa
@Temperature 121 °C
Wet
 4.10 GPa
@Temperature 24.0 °C
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 4.6
@Frequency 1e+6 Hz
ASTM D150
Dielectric Loss Index <= 0.0010
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 500 °Flight load
Glass Transition Temp, Tg 143 °C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Polyetheretherketone, Unreinforced
Ensinger Tecapeek® Polyetheretherketone (PEEK)
Solvay PEEK Laminates
Mitsubishi Chemical Advanced Materials Ketron™ 1000 PEEK, Extruded Unfilled Polyetherether Ketone
Akro-Plastic Akrotek® PEEK natural (5184) PEEK, Dry

PCYTED073 / 180375

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.