MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

A. Schulman LP544-01 High-Density Copolymer Polyethylene
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Copolymer Film Grade

Material Notes: Description

LP 544-01 is a high-density copolymer polyethylene with exceptional ESCR and crush strength combined with good processability for applications including telecommunication ducting, thermoformed parts and profile extrusions.

Information provided by A. Schulman.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.946 g/cc0.946 g/ccASTM D1505
ESCR 100% Igepal® >= 1000 hour>= 1000 hourCondition A; ASTM D1693
Melt Index of Compound 0.25 g/10 min
@Temperature 190 °C
0.25 g/10 min
@Temperature 374 °F
ASTM D1505
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 7070ASTM D2240
Tensile Strength, Yield 22.1 MPa3200 psi2"/min; ASTM D638
Elongation at Break >= 700 %>= 700 %2"/min; ASTM D638
Flexural Modulus 0.827 GPa
@Strain 2 %
120 ksi
@Strain 2 %
Secant; ASTM D790
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 65.6 °C150 °FASTM D648

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Chevron Phillips Marlex® K608 HDPE Extrusion Molding Resin
Chevron Phillips Marlex® 9346 HDPE Natural Pipe Resin
Chevron Phillips Marlex® 9512H - 9513H High Performance Series HDPE Blow Molding Resin
A. Schulman LP477-01 High-Density Polyethylene
Chevron Phillips Marlex® 9503HF High Performance Series HDPE Blow Molding Resin

PASHU084 / 25048

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.