MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Solvay BR® 95 Paste Adhesive
Categories: Polymer; Adhesive; Thermoset; Epoxy; Epoxy Adhesive

Material Notes: Description: BR® 95 paste adhesive is a two-part, modified epoxy adhesive maintaining superior strength in metallic and composite structure. BR 95 structural adhesive is curable at room temperature. Accelerated techniques may be employed if faster cure or improved elevated temperature strength are desired. To achieve consistent mechanical performance as well as maximum environmental resistance when bonding aluminum details, the use of BR® 127 corrosion inhibiting primer is recommended.

Features & Benefits:

  • Superior strength in bonding metallic and composite structures
  • Service temperature range from -67°F to 300°F (-55°C to 150°C)
  • Curable at room temperature or through accelerated curing techniques
  • Unique characteristic of a versatile mix ratio

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.935 - 0.983 g/ccPart B
 1.47 - 1.55 g/ccPart A
Solids Content 100 %Part A
 100 %Part B
Storage Temperature 12.0 °CPart A
 12.0 °CPart B
 
Mechanical PropertiesOriginal ValueComments
Shear Strength 820 psi
@Temperature 175 °C
Lap, 60 mins with BR 127 Primer at 200°F (95°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 835 psi
@Temperature 175 °C
Lap, 60 mins without Primer at 75°F (24°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 850 psi
@Temperature 175 °C
Lap, 60 mins without Primer at 200°F (95°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 890 psi
@Temperature 175 °C
Lap, 60 mins with BR 127 Primer at 75°F (24°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 1040 psi
@Temperature 175 °C
Lap, 60 mins without Primer at 75°F (24°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 1190 psi
@Temperature 150 °C
Lap, 60 mins without Primer at 75°F (24°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 1270 psi
@Temperature 175 °C
Lap, 60 mins with BR 127 Primer at 200°F (95°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 1300 psi
@Temperature 175 °C
Lap, 60 mins without Primer at 75°F (24°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 1340 psi
@Temperature 175 °C
Lap, 60 mins without Primer at 200°F (95°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 1340 psi
@Temperature 175 °C
Lap, 60 mins with BR 127 Primer at 75°F (24°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 1340 psi
@Temperature 175 °C
Lap, 60 mins with BR 127 Primer at 75°F (24°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 1360 psi
@Temperature 175 °C
Lap, 60 mins with BR 127 Primer at 200°F (95°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 1430 psi
@Temperature 150 °C
Lap, 60 mins without Primer at 200°F (95°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 1470 psi
@Temperature 150 °C
Lap, 60 mins without Primer at 200°F (95°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 1500 psi
@Temperature 150 °C
Lap, 60 mins with BR 127 Primer at 75°F (24°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 1540 psi
@Temperature 175 °C
Lap, 60 mins without Primer at 200°F (95°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 1590 psi
@Temperature -55.0 °C
Lap, 60 mins with BR 127 Primer at 75°F (24°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 1600 psi
@Temperature -55.0 °C
Lap, 60 mins without Primer at 75°F (24°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 1620 psi
@Temperature -55.0 °C
Lap, 60 mins without Primer at 75°F (24°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 1630 psi
@Temperature 150 °C
Lap, 60 mins with BR 127 Primer at 75°F (24°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 1760 psi
@Temperature 82.0 °C
Lap, 60 mins with BR 127 Primer at 75°F (24°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 1770 psi
@Temperature 150 °C
Lap, 60 mins with BR 127 Primer at 200°F (95°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 1780 psi
@Temperature 150 °C
Lap, 60 mins with BR 127 Primer at 75°F (24°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 1820 psi
@Temperature -55.0 °C
Lap, 60 mins with BR 127 Primer at 75°F (24°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 1860 psi
@Temperature 150 °C
Lap, 60 mins with BR 127 Primer at 200°F (95°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 1870 psi
@Temperature 150 °C
Lap, 60 mins without Primer at 200°F (95°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 1880 psi
@Temperature 150 °C
Lap, 60 mins with BR 127 Primer at 200°F (95°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 1900 psi
@Temperature 150 °C
Lap, 60 mins without Primer at 75°F (24°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 2140 psi
@Temperature 24.0 °C
Lap, 60 mins without Primer at 75°F (24°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 2250 psi
@Temperature 150 °C
Lap, 60 mins without Primer at 75°F (24°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 2270 psi
@Temperature 82.0 °C
Lap, 60 mins with BR 127 Primer at 75°F (24°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 2370 psi
@Temperature 82.0 °C
Lap, 60 mins without Primer at 75°F (24°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 2380 psi
@Temperature 24.0 °C
Lap, 60 mins with BR 127 Primer at 75°F (24°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 2500 psi
@Temperature 24.0 °C
Lap, 60 mins without Primer at 75°F (24°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 2510 psi
@Temperature 82.0 °C
Lap, 60 mins with BR 127 Primer at 75°F (24°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 2520 psi
@Temperature 82.0 °C
Lap, 60 mins without Primer at 200°F (95°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 2610 psi
@Temperature 24.0 °C
Lap, 60 mins with BR 127 Primer at 75°F (24°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 2730 psi
@Temperature 82.0 °C
Lap, 60 mins without Primer at 75°F (24°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 2750 psi
@Temperature 82.0 °C
Lap, 60 mins without Primer at 75°F (24°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 2770 psi
@Temperature 82.0 °C
Lap, 60 mins with BR 127 Primer at 200°F (95°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 2860 psi
@Temperature 82.0 °C
Lap, 60 mins without Primer at 200°F (95°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 2870 psi
@Temperature 24.0 °C
Lap, 60 mins without Primer at 75°F (24°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 2910 psi
@Temperature 82.0 °C
Lap, 60 mins without Primer at 200°F (95°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 2920 psi
@Temperature 24.0 °C
Lap, 60 mins without Primer at 200°F (95°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 2960 psi
@Temperature 24.0 °C
Lap, 60 mins without Primer at 200°F (95°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 2990 psi
@Temperature -55.0 °C
Lap, 60 mins with BR 127 Primer at 75°F (24°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 3080 psi
@Temperature -55.0 °C
Lap, 60 mins without Primer at 200°F (95°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 3090 psi
@Temperature 24.0 °C
Lap, 60 mins with BR 127 Primer at 75°F (24°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 3100 psi
@Temperature -55.0 °C
Lap, 60 mins without Primer at 200°F (95°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 3200 psi
@Temperature 24.0 °C
Lap, 60 mins with BR 127 Primer at 200°F (95°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 3290 psi
@Temperature 24.0 °C
Lap, 60 mins without Primer at 200°F (95°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 3300 psi
@Temperature 82.0 °C
Lap, 60 mins with BR 127 Primer at 200°F (95°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 3480 psi
@Temperature -55.0 °C
Lap, 60 mins with BR 127 Primer at 200°F (95°C), 10 psi (0.07 MPa), 10:1 Mix Ratio
 3540 psi
@Temperature 82.0 °C
Lap, 60 mins with BR 127 Primer at 200°F (95°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 3600 psi
@Temperature -55.0 °C
Lap, 60 mins with BR 127 Primer at 200°F (95°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 3680 psi
@Temperature 24.0 °C
Lap, 60 mins with BR 127 Primer at 200°F (95°C), 10 psi (0.07 MPa), 6:1 Mix Ratio
 3830 psi
@Temperature -55.0 °C
Lap, 60 mins without Primer at 200°F (95°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 3940 psi
@Temperature 24.0 °C
Lap, 60 mins with BR 127 Primer at 200°F (95°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 4120 psi
@Temperature -55.0 °C
Lap, 60 mins with BR 127 Primer at 200°F (95°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 31090 psi
@Temperature -55.0 °C
Lap, 60 mins without Primer at 75°F (24°C), 10 psi (0.07 MPa), 3:1 Mix Ratio
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 150 °C
Minimum Service Temperature, Air -55.0 °C
 
Processing PropertiesOriginal ValueComments
Cure Time 60.0 minFull Cure at 200°F (93°C)
 7200 minFull Cure at 75°F (24°C)
Pot Life >= 60.0 min100 gram mass
 300 minSet Time at 75°F (24°C)
Shelf Life 5.00 MonthPart A
 5.00 MonthPart B
 
Descriptive Properties
ColorAmberPart B
 GrayPart A

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Huntsman AroCy XU 71787.02 L Cyanate Ester
Solvay BR® 127 Primer with FM 73 Adhesive
Hexcel® HexPly® 8552 Epoxy Matrix, Carbon Fabric Form
Huntsman Araldite GY 6008 Bisphenol A Epoxy Liquid Resin
Overview of materials for Epoxy Adhesive

PCYTED124 / 180426

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.