MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Toray AMILAN™ CM1056 Nylon 6
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Unreinforced

Material Notes: Nylon 6, blow molding, high viscosity, high impact, PA6.

General Amilan™ Notes: AMILAN™ nylon (polyamide) is a thermoplastic engineering plastic containing an amide group (-CONH-) and it exhibits excellent strength, toughness, heat resistance, and anti-friction wear resistance. A variety of grades designed for various customer needs and applications are available.

Information provided by Toray Resin Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.09 g/ccDry; ISO 1183
Water Absorption 8.0 %In 23°C water, polymer initally dry; ISO 62
 1.7 %
@Time 86400 sec
In 23°C water, polymer initally dry; ISO 62
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 114
@Temperature 23.0 °C
Dry; ISO 2039-2
Tensile Strength 20.0 MPa
@Temperature 80.0 °C
3.0% Moisture Content; ISO 527-1,2
 25.0 MPa
@Temperature 80.0 °C
Dry; ISO 527-1,2
 35.0 MPa
@Temperature 23.0 °C
3.0% Moisture Content; ISO 527-1,2
 60.0 MPa
@Temperature 23.0 °C
Dry; ISO 527-1,2
 95.0 MPa
@Temperature -40.0 °C
3.0% Moisture Content; ISO 527-1,2
 105 MPa
@Temperature -40.0 °C
Dry; ISO 527-1,2
Elongation at Break 1.0 %
@Temperature -40.0 °C
3.0% Moisture Content; ISO 527-1,2
 3.5 %
@Temperature -40.0 °C
Dry; ISO 527-1,2
 50 %
@Temperature 23.0 °C
Dry; ISO 527-1,2
 50 %
@Temperature 80.0 °C
Dry; ISO 527-1,2
 50 %
@Temperature 23.0 °C
3.0% Moisture Content; ISO 527-1,2
 50 %
@Temperature 80.0 °C
3.0% Moisture Content; ISO 527-1,2
Flexural Strength 80.0 MPa
@Temperature 23.0 °C
Dry; ISO 178
 130 MPa
@Temperature -40.0 °C
Dry; ISO 178
Flexural Modulus 0.500 GPa
@Temperature 80.0 °C
Dry; ISO 178
 0.700 GPa
@Temperature 23.0 °C
3.0% Moisture Content; ISO 178
 2.10 GPa
@Temperature 23.0 °C
Dry; ISO 178
 2.90 GPa
@Temperature -40.0 °C
Dry; ISO 178
Charpy Impact Unnotched 16.0 kJ/m²
@Temperature -40.0 °C
Dry; ISO 179
 54.0 kJ/m²
@Temperature -40.0 °C
3.0% Moisture Content; ISO 179
Charpy Impact, Notched 13.5 kJ/m²
@Temperature 23.0 °C
V-Notched. Dry; ISO 179
Taber Abrasion, mg/1000 Cycles 6.0 - 7.0Dry; ISO 9352
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 50.0 - 90.0 µm/m-°CDry; ISO 11359-2
Melting Point 225 °CDry; DSC Method
Deflection Temperature at 0.46 MPa (66 psi) 160 °CDry; ISO 75-1,2
Deflection Temperature at 1.8 MPa (264 psi) 51.0 °CDry; ISO 75-1,2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PTORAY9150 / 248839

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.