MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Saint-Gobain Tygon® A-60-G Industrial Grade Tubing Formulation
Categories: Polymer; Thermoplastic

Material Notes: Norprene® Industrial Grade Tubing outperforms neoprene, EPDM and other general-purpose tubings in test after test and application after application. It will not weaken or crack after years of exposure to heat and ozone. This provides long service in a wide range of applications such as gasketing, abrasion-resistant sleeving and cable insulation. Performance formulated for on-the-job reliability, Norprene® handles temperatures from -75°F (-60°C) to 275°F (135°C), allowing the use of one material with a broad range of temperatures. It is heat sealable and can be joined without fittings. It also has excellent resistance to inorganic (acids and bases) fluids. With its outstanding flexural fatigue resistance and high temperature capability, Norprene® Industrial Grade Tubing outlasts and outperforms virtually all other general service tubings in peristaltic and vacuum pump applications.

Features/Benefits:
  • Superior weathering
  • Abrasion resistant
  • Outstanding flexural fatigue resistance
  • Wide temperature range (-75°F to 275°F)
  • Low gas permeability versus rubber tubing
  • Ozone and UV light resistant
Typical applications include Soap and Disinfectant Dispensing, Printing Ink Transfer, Caustic Dispensing, Plating and Etching Chemicals, Wastewater Sampling, Glass and Window Wash Systems, Vacuum Pumps, Cable Insulation, Abrasion Resistant Sleeving.
Information provided by Saint Gobain Performance Products.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.980 g/ccASTM D792-98
Water Absorption 0.30 %24 hours at 23°C; ASTM D570-98
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 6115 seconds; ASTM D2240-97
Tensile Strength, Yield 1000 psiASTM D412-98
Elongation at Break 375 %ASTM D412-98
100% Modulus 410 psi
@Strain 100 %
ASTM D412-98
300% Modulus 0.800 ksi
@Strain 300 %
ASTM D412-98
Tear Strength 120 pliInitial Tear Strength; ASTM D1004-94
Compression Set 27 %
@Temperature 70.0 °C
Constant Deflection, for 22 hrs.; ASTM D395-98 Method B
Tensile Set 47 %ASTM D412-98
 
Electrical PropertiesOriginal ValueComments
Dielectric Strength 535 V/milASTM D149-97
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 275 °F
Brittleness Temperature -75.0 °FASTM D746-98
 
Descriptive Properties
ColorBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Saint-Gobain Pharmed® Biocompatible Tubing for Peristaltic Pumps and Cell Culture
Saint-Gobain Tygon® A-60-F Food Process Tubing Formulation
Saint-Gobain Tygon® Noroprene® Chemical Tubing Formulation
Saint-Gobain Tygon® S3™ E-LFL Long-Flex Life Pump Tubing Formulation
Saint-Gobain Tygon® A-60-F I.B. Pressure Tubing Formulation for CIP and SIP cleaning and sterilization systems

PSTGQZ200 / 68714

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.