MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese N-277 40% Mineral Reinforced Nylon 6/6  (discontinued **)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 40% Mineral Filled

Material Notes: Description: Nylon N-277 is a 40% mineral reinforced, heat stabilized nylon 6/6 that provides excellent flatness and dimensional stability in injection molded parts. It is recommended for producing flat, low warp parts and readily fills complex shapes

Information provided by Celanese Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.50 g/cc0.0542 lb/in³ISO 1183 & ASTM D792
Moisture Absorption at Equilibrium 1.5 %1.5 %at 50% RH; ISO 62
Water Absorption at Saturation 5.1 %5.1 %ISO 62
Linear Mold Shrinkage 0.0060 cm/cm0.0060 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.010 cm/cm0.010 in/inASTM D955
Ash 40 %40 %
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 100 MPa14500 psi5 mm/min; ISO 527-2/1A
Elongation at Break 3.0 %3.0 %5 mm/min; ISO 527-2/1A
Tensile Modulus 9.90 GPa1440 ksi1 mm/min; ISO 527-2/1A
Flexural Modulus 9.30 GPa1350 ksiISO 178
Izod Impact, Notched (ISO) 3.10 kJ/m²1.48 ft-lb/in²ISO 180/1A
Charpy Impact Unnotched 3.00 J/cm²14.3 ft-lb/in²ISO 179/1eU
 2.50 J/cm²
@Temperature -30.0 °C
11.9 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched 0.300 J/cm²1.43 ft-lb/in²ISO 179/1eA
 0.280 J/cm²
@Temperature -30.0 °C
1.33 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Melting Point 257 °C495 °FASTM D3418
 263 °C505 °FISO 11357-1,2,3
Deflection Temperature at 0.46 MPa (66 psi) 240 °C464 °FISO 75-1, -2
Deflection Temperature at 1.8 MPa (264 psi) 205 °C401 °FASTM D648
 215 °C419 °FISO 75-1, -2
 
Processing PropertiesMetricEnglishComments
Melt Temperature 277 - 310 °C531 - 590 °F
Mold Temperature 60.0 - 100 °C140 - 212 °F
Drying Temperature 60.0 °C140 °F
Dry Time 1 - 2 hour1 - 2 hour
Injection Pressure 34.5 - 124 MPa5000 - 18000 psi
Back Pressure 0.000 - 0.345 MPa0.000 - 50.0 psi
Screw Speed 40 - 80 rpm40 - 80 rpm

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PHCV61 / 45902

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.