MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese Celanex® 2016 PBT, Unfilled
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes: Celanex 2016 is a non-exuding flame retarded (UL and CSA approved V-0 at 1/32 inch and 5V at 1/8 inch), unreinforced polybutylene terephthalate which has an excellent balance of mechanical properties and processability. It is well suited for electrical connector applications where UL approved 50% regrind use capability makes maximum use of purchased product.

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.44 g/ccASTM D792
Density 1.44 g/ccISO 1183
Water Absorption 0.070 %
@Temperature 22.8 °C
24hr immersion; ASTM D570
Moisture Absorption 0.170 %23°C/50%RH; ISO 62
Linear Mold Shrinkage, Flow 0.012 - 0.016 cm/cmISO 294-4
 0.025 - 0.030 cm/cmASTM D955
Linear Mold Shrinkage, Transverse 0.012 - 0.016 cm/cmISO 294-4
Melt Flow 25 g/10 minASTM D1238
 18 g/10 min
@Load 2.16 kg,
Temperature 250 °C
[cm3/10min]; ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 79ISO 2039-2
Tensile Strength, Yield 60.0 MPa50mm/min; ISO 527-2/1A
 8600 psiASTM D638
Elongation at Break 10 %
 20 %ASTM D638
Elongation at Yield 3.0 %50mm/min; ISO 527-2/1A
Tensile Modulus 3000 MPa50mm/min; ISO 527-2/1A
Flexural Strength 95.0 MPaISO 178
 15400 psiASTM D790
Flexural Modulus 3100 MPaISO 178
 477000 psiASTM D790
Izod Impact, Notched 0.600 ft-lb/inASTM D256
Izod Impact, Notched (ISO) 4.50 kJ/m²ISO 180/1A
Charpy Impact Unnotched 55.0 kJ/m²ISO 179/1eU
 55.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
Charpy Impact, Notched 4.00 kJ/m²ISO 179/1eA
 4.50 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmIEC 60093
 2.00e+16 ohm-cmASTM D257
Surface Resistance 1.00e+15 ohmIEC 60093
Dielectric Constant 3.0
@Frequency 1e+6 Hz
ASTM D150
 3.5
@Frequency 1e+6 Hz
IEC 60250
 3.6
@Frequency 100 Hz
IEC 60250
Dielectric Strength 25.0 kV/mmIEC 60243-1
 700 V/milshort term; ASTM D149
Dissipation Factor 0.0047
@Frequency 100 Hz
IEC 60250
 0.010
@Frequency 1e+6 Hz
ASTM D150
 0.0185
@Frequency 1e+6 Hz
IEC 60250
Arc Resistance 96 secASTM D495
Comparative Tracking Index 250 VIEC 60112
 325 VASTM D3638
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 63.0 µm/m-°CISO 11359-2
CTE, linear, Transverse to Flow 77.0 µm/m-°CISO 11359-2
Melting Point 225 °C10°C/min; ISO 11357-1,-2,-3
 437 °FASTM D3418
Deflection Temperature at 0.46 MPa (66 psi) 165 °CISO 75-1, -2
 328 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 68.0 °CISO 75-1, -2
 158 °FASTM D648
Vicat Softening Point 190 °CISO 306
Glass Transition Temp, Tg 60.0 °CISO 11357-1,-2,-3
Flammability, UL94 V-0
 5VA
@Thickness 3.00 mm
Oxygen Index 30 %ISO 4589
 
Processing PropertiesOriginal ValueComments
Processing Temperature 65.0 - 93.0 °Ccavity
 250 - 260 °Chot runner
Feed Temperature 230 - 240 °C
Zone 1 230 - 240 °C
Zone 2 235 - 250 °C
Zone 3 235 - 250 °C
Zone 4 240 - 255 °C
Die Temperature 250 - 255 °C
Melt Temperature 243 °CISO 294
 235 - 255 °C
Mold Temperature 82.0 °CISO 294
Injection Velocity 300 mm/secISO 294
Drying Temperature 120 - 130 °C
Dry Time 4.00 hour
Moisture Content <= 0.020 %
Hold Pressure 48.0 MPaISO 294
 
Descriptive Properties
Injection moldingYes
Injection speedmedium-fast
Processing conditions acc. ISO7792-2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Ultramid® 1000-2 NF2001 PA66 (Dry)
Celanese Celanex® 3216 PBT, 15% Glass Reinforced
BASF Ultradur® B 4406 G4 PBT
Celanese Celanex® 3316 PBT, 30% Glass Reinforced
Syensqo (Solvay Specialty Polymers) Mindel® B-430 Polysulfone, Modified (PSU, Modified)

PHCQ022 / 178477

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.