MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
AISI 4140 Steel, oil quenched, 315°C (600°F) temper, 25 mm (1 in.) round
Categories: Metal; Ferrous Metal; Alloy Steel; AISI 4000 Series Steel; Low Alloy Steel; Carbon Steel; Medium Carbon Steel

Material Notes: As quenched hardness after oil quenching: Surface - 55 HRC, 1/2 radius - 55 HRC; Center - 50 HRC

Key Words: ASTM A322, ASTM A331, ASTM A505, ASTM A519, ASTM A646, B.S. 708 A 42 (UK), B.S. 708 M 40 (UK), B.S. 709 M 40 (UK), JIS SCM 4 H, JIS SCM 4, JIS SCM440, SS14 2244 (Sweden), MIL SPEC MIL-S-16974, SAE J404, SAE J412, SAE J770, DIN 1.7225, UNS G41400, AMS 6381, AMS 6382, AMS 6390, AMS 6395, IS 1570 40Cr1Mo28, IS 4367 40Cr1Mo28, IS 5517 40Cr1Mo28
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.85 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 455
Hardness, Knoop 488Converted from Brinell
Hardness, Rockwell B 110Converted from Brinell hardness. Beyond normal Rockwell B hardness range, for comparison only.
Hardness, Rockwell C 48Converted from Brinell
Hardness, Vickers 482Converted from Brinell
Tensile Strength, Ultimate 1585 MPa
Tensile Strength, Yield 1345 MPa
Elongation at Break 11 %
Reduction of Area 40 %
Modulus of Elasticity 205 GPaTypical for steel
Bulk Modulus 160 GPaTypical for steel
Poissons Ratio 0.29Calculated
Machinability 65 %Based on AISI 1212 as 100% machinability.
Shear Modulus 80.0 GPaTypical for steel
Izod Impact 9.00 J
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000220 ohm-cm
@Temperature 20.0 °C
specimen hardened and tempered
 0.0000263 ohm-cm
@Temperature 100 °C
specimen hardened and tempered
 0.0000326 ohm-cm
@Temperature 200 °C
specimen hardened and tempered
 0.0000475 ohm-cm
@Temperature 400 °C
specimen hardened and tempered
 0.0000646 ohm-cm
@Temperature 600 °C
specimen hardened and tempered
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.2 µm/m-°C
@Temperature 0.000 - 100 °C
 13.7 µm/m-°C
@Temperature 20.0 - 400 °C
 14.6 µm/m-°C
@Temperature 20.0 - 600 °C
Specific Heat Capacity 0.473 J/g-°C
@Temperature 150 - 200 °C
 0.519 J/g-°C
@Temperature 350 - 400 °C
 0.561 J/g-°C
@Temperature 550 - 600 °C
Thermal Conductivity 42.6 W/m-K
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.38 - 0.43 %
Chromium, Cr 0.80 - 1.1 %
Iron, Fe 96.785 - 97.77 %As remainder
Manganese, Mn 0.75 - 1.0 %
Molybdenum, Mo 0.15 - 0.25 %
Phosphorus, P <= 0.035 %
Silicon, Si 0.15 - 0.30 %
Sulfur, S <= 0.040 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 4140 Steel, oil quenched, 425°C (800°F) temper, 25 mm (1 in.) round
AISI 4140 Steel, oil quenched, 205°C (400°F) temper, 25 mm (1 in.) round
AISI 4140 Steel, oil quenched, 650°C (1200°F) temper, 25 mm (1 in.) round
AISI 4140 Steel, oil quenched, 540°C (1000°F) temper, 25 mm (1 in.) round
AISI 4140 Steel, annealed at 815°C (1500°F) furnace cooled 11°C (20°F)/hour to 665°C (1230°F), air cooled, 25 mm (1 in.) round

M4140S / 7546

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.