MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Overview of materials for Polybutene
Categories: Polymer; Thermoplastic; Polybutene

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polybutene". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.870 - 0.918 g/ccAverage value: 0.902 g/cc Grade Count:36
Viscosity 3200 - 640000 cP
@Temperature 117 - 190 °C
Average value: 135000 cP Grade Count:7
Environmental Stress Crack Resistance >= 15000 hour
@Temperature 50.0 - 50.0 °C
Average value: 15000 hour Grade Count:3
Melt Flow 0.400 - 2500 g/10 minAverage value: 191 g/10 min Grade Count:36
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 12.0 - 35.0 MPaAverage value: 27.2 MPa Grade Count:22
Film Tensile Strength at Yield, MD 15.0 - 23.0 MPaAverage value: 19.0 MPa Grade Count:3
Tensile Strength, Yield 3.74 - 17.2 MPaAverage value: 10.6 MPa Grade Count:8
Film Elongation at Break, MD 580 - 790 %Average value: 708 % Grade Count:5
Elongation at Break 300 - 800 %Average value: 343 % Grade Count:21
Modulus of Elasticity 0.0517 - 0.293 GPaAverage value: 0.163 GPa Grade Count:10
Flexural Modulus 0.0100 - 0.450 GPaAverage value: 0.240 GPa Grade Count:19
Secant Modulus, MD 0.185 - 0.550 GPaAverage value: 0.315 GPa Grade Count:5
Film Tensile Strength at Break, MD 28.0 - 34.0 MPaAverage value: 31.0 MPa Grade Count:5
 
Thermal PropertiesOriginal ValueComments
Melting Point 81.0 - 128 °CAverage value: 106 °C Grade Count:25
Vicat Softening Point 90.0 - 113 °CAverage value: 102 °C Grade Count:8
Brittleness Temperature -34.0 - -17.0 °CAverage value: -22.7 °C Grade Count:7

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Molded
Overview of materials for Polybutylene Terephthalate (PBT), Unreinforced, Molded
Overview of materials for Polyamide-Imide, Molded
Overview of materials for Polybutylene Terephthalate (PBT), Extrusion Grade
Overview of materials for Polycarbonate, Molded

O2995 / 77779

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.