MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
LG Chemical ALPHALAC SF510 HIPS
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene, Impact Grade, Glass Filled

Material Notes: Super flow, High gloss and high impact equivalent to ABS, Excellent mechanical properties compare with general HIPS, Meet requirements for cost and quality, Applications include TV cabinets, thin part, and high speed injection molding

CAS No. 9003-55-8

Information provided by LG Chemical

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.04 g/ccASTM D792
Maximum Moisture Content 0.010Injection Molding
Melt Flow 12 g/10 min
@Load 5.00 kg,
Temperature 200 °C
ASTM D1238(G)
 34 g/10 min
@Load 3.80 kg,
Temperature 230 °C
ASTM D1238(I)
 137 g/10 min
@Load 10.0 kg,
Temperature 220 °C
ASTM D1238(G)
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 101ASTM D785
Tensile Strength, Yield 270 kg(f)/cm²
@Thickness 3.20 mm
50mm/min; ASTM D638
Elongation at Break 51 %
@Thickness 3.20 mm
50mm/min; ASTM D638
Elongation at Yield 5.0 %
@Thickness 3.20 mm
50mm/min; ASTM D638
Tensile Modulus 21500 kg(f)/cm²
@Thickness 3.20 mm
1mm/min; ASTM D638
Flexural Yield Strength 430 kg(f)/cm²
@Thickness 3.20 mm
15mm/min; ASTM D790
Flexural Modulus 23500 kg(f)/cm²
@Thickness 3.20 mm
15mm/min; ASTM D790
Izod Impact, Notched 5.00 kg-cm/cm
@Thickness 6.50 mm,
Temperature -30.0 °C
ASTM D256
 7.00 kg-cm/cm
@Thickness 3.20 mm,
Temperature -30.0 °C
ASTM D256
 10.0 kg-cm/cm
@Thickness 6.50 mm,
Temperature 23.0 °C
ASTM D256
 14.0 kg-cm/cm
@Thickness 3.20 mm,
Temperature 23.0 °C
ASTM D256
 
Electrical PropertiesOriginal ValueComments
Arc Resistance 60 - 120 secASTM D495
Comparative Tracking Index 400 - 600 V
Hot Wire Ignition, HWI 7.0 - 15 sec
@Thickness >=1.50 mm
 15 - 30 sec
@Thickness >=3.00 mm
High Amp Arc Ignition, HAI 60 - 120 arcs
@Thickness 1.50 mm
 60 - 120 arcs
@Thickness 3.00 mm
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 89.0 °C
@Thickness 6.40 mm
Unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 80.0 °C
@Thickness 6.40 mm
Unannealed; ASTM D648
Vicat Softening Point 88.0 °C
@Load 5.00 kg
50°C/h; ASTM D1525
UL RTI, Electrical 50.0 °C
@Thickness >=1.50 mm
 50.0 °C
@Thickness >=3.00 mm
UL RTI, Mechanical with Impact 50.0 °C
@Thickness >=1.50 mm
 50.0 °C
@Thickness >=3.00 mm
UL RTI, Mechanical without Impact 50.0 °C
@Thickness >=1.50 mm
 50.0 °C
@Thickness >=3.00 mm
Flammability, UL94 HB
@Thickness >=1.50 mm
 HB
@Thickness >=3.00 mm
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 170 - 190 °CInjection Molding
Middle Barrel Temperature 180 - 200 °CInjection Molding
Front Barrel Temperature 190 - 210 °CInjection Molding
Nozzle Temperature 190 - 220 °CInjection Molding
Melt Temperature 190 - 220 °CInjection Molding
Mold Temperature 40.0 - 70.0 °CInjection Molding
Drying Temperature 80.0 °CInjection Molding
Dry Time 2.00 - 4.00 hourInjection Molding
Back Pressure 29.4 - 58.8 MPaInjection Molding
Screw Speed 30 - 60 rpmInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
LG Chemical ALPHALAC SG960 HIPS
INEOS Styrolution PS 485N HIPS
LG Chemical ALPHALAC SG910 HIPS
Ineos Nova 464 High Impact Polystyrene Injection Molding Grade
Eastman Eastar 6763 PETG Copolyester

PLAY256 / 148266

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.