MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Celstran® PPS-GF30-01 PPS, 30% Glass Reinforced
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS); Polyphenylene Sulfide (PPS) with 30% Glass Fiber Filler

Material Notes: 30% long strand fiber glass reinforced polyphenylene sulfide
30% long strand glass fiber reinforced polyphenylene sulfide

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.52 g/cc1.52 g/ccASTM D792
Density 1.45 g/cc0.0524 lb/in³ISO 1183
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 165 MPa23900 psiASTM D638
 173 MPa
@Temperature -40.0 °C
25100 psi
@Temperature -40.0 °F
ASTM D638
Elongation at Break  1.3 %
@Temperature -40.0 °C
1.3 %
@Temperature -40.0 °F
ASTM D638
 1.3 %
@Temperature 22.8 °C
1.3 %
@Temperature 73.0 °F
ASTM D638
Tensile Modulus  13.2 GPa
@Temperature 22.8 °C
1910 ksi
@Temperature 73.0 °F
ASTM D638
 15.2 GPa
@Temperature -40.0 °C
2200 ksi
@Temperature -40.0 °F
ASTM D638
Flexural Strength 229 MPa33200 psiASTM D790
 234 MPa
@Temperature -40.0 °C
34000 psi
@Temperature -40.0 °F
ASTM D790
Flexural Modulus  11.6 GPa
@Temperature 22.8 °C
1680 ksi
@Temperature 73.0 °F
ASTM D790
 12.1 GPa
@Temperature -40.0 °C
1760 ksi
@Temperature -40.0 °F
ASTM D790
Izod Impact, Notched 3.15 J/cm5.90 ft-lb/inASTM D256
 3.20 J/cm
@Temperature -40.0 °C
6.00 ft-lb/in
@Temperature -40.0 °F
ASTM D256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 254 °C490 °FASTM D648
 
Processing PropertiesMetricEnglishComments
Processing Temperature 70.0 - 80.0 °C158 - 176 °F
 140 - 160 °C284 - 320 °FCavity temperature
Feed Temperature 20.0 - 50.0 °C68.0 - 122 °F
Zone 1 285 - 295 °C545 - 563 °F
Zone 2 290 - 300 °C554 - 572 °F
Zone 3 295 - 305 °C563 - 581 °F
Zone 4 300 - 310 °C572 - 590 °F
Die Temperature 290 - 300 °C554 - 572 °F
Melt Temperature 300 - 310 °C572 - 590 °F
Drying Temperature 130 - 140 °C266 - 284 °F
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hour
Moisture Content 0.020 %0.020 %Necessary low maximum residual
Dew Point <= -30.0 °C<= -22.0 °FPre-drying
 
Descriptive Properties
Longer pre-drying times/storagelower the temperature to 100° C until processed.<= 60 h

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese FORTRON 1130L0 PPS, 30% Glass Reinforced
Celanese FORTRON 1130L4 PPS, 30% Glass Reinforced
Albis Plastics Tedur® L V 9404-1 PPS, 30% Carbon Fiber
Techmer ES Luriblend® PPS GF30 TL15 30% Glass Filled
Celanese Celstran® PPS-CF30-01 PPS, 30% Specialty

PHCR224 / 158793

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.