MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Chevron Phillips Marlex® 1007 Injection Molding Resin
Categories: Polymer; Thermoplastic; Polyethylene (PE); Low Density (LDPE); Low Density Polyethylene (LDPE), Molded

Material Notes: This autoclave LDPE homopolymer is tailored for applications that require:
  • Excellent flexibility
  • Good flow
  • Good warpage resistance
Typical injection molded applications for 1007 include:
  • Housewares
  • Tamper evident, snap-on caps
  • Wine bottle sleeve caps
This resin meets these specifications:
  • ASTM D4976 - PE 113
  • FDA 21 CFR 177.1520(c) 2.2, use conditions B through H per 21 CFR 176.170(c)

Data provided by Chevron Chemical.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.917 g/ccASTM D1505
Melt Flow 7.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D 1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 47ASTM D2240
Tensile Strength, Yield 9.00 MPa2 in/min, Type IV bar; ASTM D638
Elongation at Break 600 %2 in/min, Type IV bar; ASTM D638
Flexural Modulus 0.200 GPaTangent - 16:1 span:depth, 0.5 in/min; ASTM D790
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 87.0 °CLoading 1, Rate A; ASTM D1525
Brittleness Temperature -66.0 °CType A, Type I specimen; ASTM D746
 
Compliance PropertiesOriginal ValueComments
FDA YesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chevron Phillips Marlex® 1003 LDPE Injection Molding Resin
Chevron Phillips Marlex® 1122B Injection Molding Resin
Chevron Phillips Marlex® 1009 LDPE Injection Molding Resin
Bamberger Polymers Bapolene® 2272 Polyethylene, Injection Grade
Chevron Phillips Marlex® 1412 Injection Molding Resin

PCHEVV04 / 20400

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.