MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Arkema KYNAR FLEX® 2850-07 Polyvinylidene Fluoride Copolymer - Extrusion & Molding
Categories: Polymer; Thermoplastic; Fluoropolymer; Polyvinylidene Fluoride (PVDF); Polyvinylidinefluoride (PVDF), Molded/Extruded

Material Notes: Characteristics: Natural resin - translucent, off-white hemispheres. 150°C Temperature rating. High stability in harsh thermal, chemical and ultraviolet environments. High toughness and mechanical strength, low permeability, abrasion resistance; high purity

Applications:

  • Chemical processing – production, storage and transfer of corrosive fluids
  • Electronics – protective sheathing, plenum and wiring insulation
  • Semi-conductor industry
  • Food stuff and Healthcare industries
  • Transportation – fuel line and pipe, thermoformed body components

Information provided by Arkema Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.77 - 1.80 g/cc1.77 - 1.80 g/ccASTM D792
Density 1.77 g/cc0.0639 lb/in³ISO 1183
Water Absorption 0.030 %0.030 %Dry; Sim. to ISO 62
Viscosity 1.60e+6 - 2.00e+6 cP
@Shear Rate 100 1/s,
Temperature 230 °C
1.60e+6 - 2.00e+6 cP
@Shear Rate 100 1/s,
Temperature 446 °F
Melt; ASTM D3835
Melt Flow 9.0 - 16 g/10 min
@Load 12.5 kg,
Temperature 230 °C
9.0 - 16 g/10 min
@Load 27.6 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 70 - 7570 - 75ASTM D2240
Tensile Strength at Break 27.6 - 48.3 MPa4000 - 7010 psiASTM D638
Tensile Strength, Yield 31.0 - 41.4 MPa4500 - 6000 psiASTM D638
 40.0 MPa5800 psiDry; ISO 527-1/-2
Elongation at Break >= 50 %>= 50 %Dry; ISO 527-1/-2
 30 - 200 %30 - 200 %ASTM D638
Elongation at Yield 5.0 - 15 %5.0 - 15 %ASTM D638
 11 %11 %Dry; ISO 527-1/-2
Tensile Modulus 1.03 - 1.52 GPa149 - 220 ksiASTM D638
 1.30 GPa189 ksiDry; ISO 527-1/-2
Flexural Strength 20.7 - 34.5 MPa
@Strain 5.0 %
3000 - 5000 psi
@Strain 5.0 %
ASTM D790
Flexural Modulus 1.03 - 1.24 GPa149 - 180 ksiASTM D790
Compressive Strength 41.4 - 58.6 MPa6000 - 8500 psiASTM D695
Izod Impact, Notched 1.60 - 4.27 J/cm3.00 - 8.00 ft-lb/inASTM D256
Izod Impact, Unnotched NBNBASTM D256
Charpy Impact, Notched NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Dry; ISO 179/1eA
Coefficient of Friction, Dynamic 0.190.19vs. steel; ASTM D1894
Coefficient of Friction, Static 0.260.26vs. steel; ASTM D1894
Taber Abrasion, mg/1000 Cycles 6.0 - 9.06.0 - 9.0CS 17 1000g:pad; ASTM-G195-13A
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 2.00e+14 ohm-cm2.00e+14 ohm-cm65% R.H; ASTM D257
 2.00e+14 ohm-cm2.00e+14 ohm-cmDry; IEC 60093
Dielectric Constant  3.5 - 10.2
@Frequency 1000 Hz
3.5 - 10.2
@Frequency 1000 Hz
ASTM D150
 6.85
@Frequency 100 Hz
6.85
@Frequency 100 Hz
Dry; IEC 60250
Dielectric Strength 1.40 kV/mm35.6 kV/inDry; IEC 60243-1
 1.30 - 1.60 kV/mm33.0 - 40.6 kV/inASTM D149
Dissipation Factor  0.000012
@Frequency 100 Hz
0.000012
@Frequency 100 Hz
Dry; IEC 60250
 0.010 - 0.22
@Frequency 100000 Hz
0.010 - 0.22
@Frequency 100000 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 126 - 185 µm/m-°C70.0 - 103 µin/in-°FASTM D696
Specific Heat Capacity 0.745 - 0.958 J/g-°C0.178 - 0.229 BTU/lb-°FDSC
Thermal Conductivity 0.144 - 0.180 W/m-K0.999 - 1.25 BTU-in/hr-ft²-°FASTM D433
Melting Point 157 °C315 °F10°C/min; Dry; ISO 11357-1/-3
 155 - 160 °C311 - 320 °FASTM D3418
Maximum Service Temperature, Air 140 °C284 °FUL RTI
Deflection Temperature at 0.46 MPa (66 psi) 60.0 - 75.0 °C140 - 167 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 37.8 - 55.0 °C100 - 131 °FASTM D648
Glass Transition Temp, Tg -40.6 - -38.3 °C-41.1 - -36.9 °FASTM D7028
Decomposition Temperature 375 °C707 °F1% wt. loss, TGA, in air
 410 °C770 °F1% wt. loss, TGA, in nitrogen
UL RTI, Electrical 140 °C284 °FUL 746B
UL RTI, Mechanical without Impact 140 °C284 °FUL 746B
Flammability, UL94  V-0
@Thickness 0.800 mm
V-0
@Thickness 0.0315 in
IEC 60695-11-10
 V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
Yellow Card Available; Dry; IEC 60695-11-10
Oxygen Index 43 %43 %ASTM D2863
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.421.42sodium D line; ASTM D542
 
Descriptive Properties
Moisture SensitiveNo

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Arkema Kynar Flex® PPA 2200 PVDF
Arkema KYNAR FLEX® 3120-50 Polyvinylidene Fluoride Copolymer - Extrusion & Molding
Arkema KYNAR FLEX® 2800-20 Polyvinylidene Fluoride Copolymer - Extrusion & Molding
Arkema KYNAR FLEX® 2950-05 Polyvinylidene Fluoride Copolymer - Extrusion & Molding
Arkema Kynar Flex® Ultraflex B PVDF

PARKG921 / 144546

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.