MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Constellium DOKIMA® Rolled Plate Aluminum
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 6000 Series Aluminum Alloy

Material Notes: DOKIMA® rolled plates have moderate strength properties, a very low level of impurities, an excellent corrosion resistance, a very good dimensional stability and high thermal and electrical conductivity. DOKIMA® is recommended for sensitive applications in nuclear, pharmaceutical, food, semi-conductor and telecommunication industries.

Information provided by manufacturer

Key Words: Alloy 6063S
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.69 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 100
@Thickness 8.00 - 25.0 mm
 100
@Thickness 25.0 - 60.0 mm
 100
@Thickness 60.0 - 100 mm
 100
@Thickness 100 - 150 mm
Tensile Strength >= 260 MPa
@Thickness 8.00 - 25.0 mm
Temper T651
 >= 260 MPa
@Thickness 25.0 - 60.0 mm
Temper T651
 >= 260 MPa
@Thickness 60.0 - 150 mm
Temper T651
 300 MPa
@Thickness 8.00 - 25.0 mm
Typical Strength
 300 MPa
@Thickness 25.0 - 60.0 mm
Typical Strength
 300 MPa
@Thickness 60.0 - 100 mm
Typical Strength
 300 MPa
@Thickness 100 - 150 mm
Typical Strength
Tensile Strength, Yield >= 220 MPa
@Strain 0.2 %,
Thickness 8.00 - 25.0 mm
Temper T651
 >= 220 MPa
@Strain 0.2 %,
Thickness 25.0 - 60.0 mm
Temper T651
 >= 220 MPa
@Strain 0.2 %,
Thickness 60.0 - 150 mm
Temper T651
 260 MPa
@Strain 0.2 %,
Thickness 8.00 - 25.0 mm
Typical Strength
 260 MPa
@Strain 0.2 %,
Thickness 25.0 - 60.0 mm
Typical Strength
 260 MPa
@Strain 0.2 %,
Thickness 60.0 - 100 mm
Typical Strength
 260 MPa
@Strain 0.2 %,
Thickness 100 - 150 mm
Typical Strength
Elongation at Break >= 5.0 %
@Thickness 60.0 - 150 mm
Temper T651
 >= 6.0 %
@Thickness 25.0 - 60.0 mm
Temper T651
 >= 7.0 %
@Thickness 8.00 - 25.0 mm
Temper T651
 8.0 %
@Thickness 100 - 150 mm
Typical Elongation
 9.0 %
@Thickness 60.0 - 100 mm
Typical Elongation
 10 %
@Thickness 8.00 - 25.0 mm
Typical Elongation
 10 %
@Thickness 25.0 - 60.0 mm
Typical Elongation
Modulus of Elasticity 68.3 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000340 ohm-cmTemper T651
 
Thermal PropertiesOriginal ValueComments
CTE, linear 23.4 µm/m-°C
@Temperature 20.0 - 100 °C
Thermal Conductivity 200 W/m-KTemper T651
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 97.65 - 99.35 %as balance
Chromium, Cr <= 0.10 %
Copper, Cu <= 0.10 %
Iron, Fe <= 0.35 %
Magnesium, Mg 0.45 - 0.90 %
Manganese, Mn <= 0.10 %
Silicon, Si 0.20 - 0.60 %
Titanium, Ti <= 0.10 %
Zinc, Zn <= 0.10 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Superior Flux Superior No. 40MM4 Organic Acid Water-Soluble Flux
Arkema KYNAR® 370 Polyvinylidene Fluoride (PVDF) Homopolymer - Injection Molding
Aluminum 6061-T6; 6061-T651
Goodfellow Aluminum 99/Silicon 1 Alloy
Alpase M-5™ Aluminum Mold Plate

NCONS019 / 160282

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.