System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
Mitsubishi Rayon ACRYPET VR L40 001 PMMA Resin
Categories:
Polymer
;
Thermoplastic
;
Acrylic (PMMA)
;
Acrylic, Impact Modified, Molded
Material Notes:
Standard type of top-grade Impact strength.
Typical Products: Interior parts of Auto mobile and Audio system. Indicator window of mobile phone.
Information provided by Mitsubishi Rayon Co.,Ltd.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Specific Gravity
1.16
g/cc
ISO 1183; JIS K7112
Water Absorption
0.30 %
@Time 86400 sec
ISO 62
Linear Mold Shrinkage
0.0030
-
0.0070
cm/cm
MRC method
Melt Flow
2.3
g/10 min
@Load 3.80 kg,
Temperature 230 °C
ISO 1133
Spiral Flow
130
cm
@Thickness 2.00 mm,
Temperature 250 °C
MRC method
220
cm
@Thickness 2.00 mm,
Temperature 250 °C
MRC method
Mechanical Properties
Original Value
Comments
Hardness, Rockwell M
69
ISO 2039
Tensile Strength
52.0
MPa
1A/5; ISO 527
Elongation at Break
30 %
1A/5; ISO 527
Modulus of Elasticity
2.00
GPa
1A/1; ISO 527
Flexural Strength
78.0
MPa
ISO 178
Flexural Modulus
2.00
GPa
ISO 178
Izod Impact, Unnotched (ISO)
9.20
kJ/m²
1A; ISO 180
Charpy Impact Unnotched
140
kJ/m²
11eU; ISO 179
Charpy Impact, Notched
7.40
kJ/m²
1eA; ISO 179
Electrical Properties
Original Value
Comments
Volume Resistivity
>=
1e+12
ohm-cm
JIS K6911
Surface Resistance
>=
1.00e+16
ohm
JIS K6911
Dielectric Constant
3.7
@Frequency 60 Hz
JIS K6911
Dielectric Strength
20.0
kV/mm
4kV/sec; JIS K6911
Dissipation Factor
0.050
@Frequency 60 Hz
JIS K6911
Thermal Properties
Original Value
Comments
CTE, linear
90.0
µm/m-°C
ASTM D696
Specific Heat Capacity
1.50
J/g-°C
JIS K7123
Thermal Conductivity
0.200
W/m-K
ASTM C177
Deflection Temperature at 1.8 MPa (264 psi)
94.0
°C
ISO 75
Vicat Softening Point
99.0
°C
@Load 5.10 kg
ISO 75
Optical Properties
Original Value
Comments
Refractive Index
1.49
@Wavelength 587.6 nm
n
d
; ASTM D542
Haze
0.50 %
@Thickness 3.00 mm
ISO 14782
Transmission, Visible
92 %
@Thickness 3.00 mm
ISO 13468
Descriptive Properties
Arc Resistance
no track
JIS K6911
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
Users viewing this material also viewed the following:
Mitsubishi Rayon Acrypet® VH-001 Heat Stabilized PMMA
Mitsubishi Rayon ACRYPET VH 000 PMMA Resin
Röhm Plexiglas® 8N PMMA Molding Compound
Röhm Plexiglas® zk5BR Molding Compound
Röhm Plexiglas® zk6BR Molding Compound
PMITS9913 / 185888
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.