System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
Aperam N485 Cold Rolled Strip
Categories:
Metal
;
Ferrous Metal
Material Notes:
N485 is an iron-nickel chromium controlled expansion alloy suitable to soft glass sealing, with optimal chemical composition to obtain hermetic seals.
International standards: DIN 17745 - W 2.4486 - SEW 385
Information provided by Aperam
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Density
8.20
g/cc
Mechanical Properties
Original Value
Comments
Hardness, Vickers
140
Annealed
230
Hard Temper
Tensile Strength, Ultimate
540
MPa
Annealed
730
MPa
Hard Temper
Tensile Strength, Yield
250
MPa
Annealed
700
MPa
Hard Temper
Elongation at Break
4.0 %
Hard Temper
35 %
Annealed
Tensile Modulus
160000
MPa
Young's, Annealed
Electrical Properties
Original Value
Comments
Volume Resistivity
0.000085
ohm-cm
Curie Temperature
350
°C
Thermal Properties
Original Value
Comments
CTE, linear
9.90
-
10.7
µm/m-°C
@Temperature 30.0 - 400 °C
Specific Heat Capacity
0.500
J/g-°C
Thermal Conductivity
14.2
W/m-K
Melting Point
1450
°C
Component Elements Properties
Original Value
Comments
Cobalt, Co
6.0 %
Iron, Fe
46.5 %
Nickel, Ni
47.5 %
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
Users viewing this material also viewed the following:
Aperam Invar® Controlled Expansion Alloys Iron-Nickel Alloys
Aperam FeNi 70 Controlled Expansion Alloys Iron-Nickel Alloys
Aperam N42 Cold Rolled Strip
Aperam N475 Cold Rolled Strip
Latrobe MP35N® Alloy
NPERA044 / 194833
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.