MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Aluminum 6061-T91
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 6000 Series Aluminum Alloy

Material Notes: Information provided by Alcoa and the references. General 6061 characteristics and uses: Excellent joining characteristics, good acceptance of applied coatings. Combines relatively high strength, good workability, and high resistance to corrosion; widely available. The T8 and T9 tempers offer better chipping characteristics over the T6 temper.

Uses: Aircraft fittings, camera lens mounts, couplings, marines fittings and hardware, electrical fittings and connectors, decorative or misc. hardware, hinge pins, magneto parts, brake pistons, hydraulic pistons, appliance fittings, valves and valve parts.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: al6061, UNS A96061; ISO AlMg1SiCu; Aluminium 6061-T91, AD-33 (Russia); AA6061-T91; Al6061-T91
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.70 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 108500 kg load with 10 mm ball. Calculated value.
Hardness, Knoop 137Converted from Brinell Hardness Value
Hardness, Rockwell A 44.1Converted from Brinell Hardness Value
Hardness, Rockwell B 69Converted from Brinell Hardness Value
Hardness, Vickers 123Converted from Brinell Hardness Value
Tensile Strength, Ultimate 405 MPa
Tensile Strength, Yield 395 MPa
Elongation at Break 12 %In 5 cm; Sample 1.6 mm thick
Modulus of Elasticity 69.0 GPaAverage of Tension and Compression. In Al alloys, the compressive modulus is typically 2% greater than the tensile modulus
Poissons Ratio 0.33Estimated from trends in similar Al alloys.
Fatigue Strength 95.0 MPa
@# of Cycles 5.00e+8
Shear Modulus 26.0 GPaEstimated from similar Al alloys.
Shear Strength 230 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000400 ohm-cmEstimated from other heat treatments.
 
Thermal PropertiesOriginal ValueComments
CTE, linear 13.1 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 25.2 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.896 J/g-°C
Thermal Conductivity 170 W/m-KEstimated from other heat treatments.
Melting Point 1080 - 1205 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting can be eliminated by homogenization.
Solidus 1080 °FAA; Typical
Liquidus 1205 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Solution Temperature 985 °F
Aging Temperature 320 °FRolled or drawn products; hold at temperature for 18 hr
 350 °FExtrusions or forgings; hold at temperature for 8 hr
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 95.8 - 98.6 %As remainder
Chromium, Cr 0.04 - 0.35 %
Copper, Cu 0.15 - 0.40 %
Iron, Fe <= 0.70 %
Magnesium, Mg 0.80 - 1.2 %
Manganese, Mn <= 0.15 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si 0.40 - 0.80 %
Titanium, Ti <= 0.15 %
Zinc, Zn <= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 6061-T6; 6061-T651
Aluminum 6061-T8
Aluminum 6061-T4; 6061-T451
Aluminum 6061-T913
Aluminum 6061-O

MA6061T91 / 9393

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.