MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Erbslöh Aluminium DISPAL S693 Aluminum Alloy, AlCu5Ti, Condition T4
Categories: Metal; Nonferrous Metal; Aluminum Alloy

Material Notes: High stiffness and elongation at rupture. Property data for Condition T4 (Quench in water at RT).

Information provided by PEAK Werkstoff GmbH, a part of Erbslöh Aluminium GmbH.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.679 - 2.961 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers >= 125
Tensile Strength >= 488 MPa
Tensile Strength, Yield >= 334 MPa
Elongation at Break >= 16 %
Modulus of Elasticity >= 72.0 GPa
 >= 58.0 GPa
@Temperature 300 °C
Condition T6
 >= 65.0 GPa
@Temperature 200 °C
Condition T6
Poissons Ratio 0.341
@Temperature 20.0 °C
Condition T6
 0.347
@Temperature 100 °C
Condition T6
 0.354
@Temperature 150 °C
Condition T6
 0.361
@Temperature 200 °C
Condition T6
 0.364
@Temperature 250 °C
Condition T6
 0.369
@Temperature 300 °C
Condition T6
Shear Modulus 23.0 GPa
@Temperature 300 °C
Condition T6
 24.0 GPa
@Temperature 200 °C
Condition T6
 24.0 GPa
@Temperature 250 °C
Condition T6
 25.0 GPa
@Temperature 150 °C
Condition T6
 26.0 GPa
@Temperature 100 °C
Condition T6
 28.0 GPa
@Temperature 20.0 °C
Condition T6
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000570 - 0.00000610 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 22.9 - 23.9 µm/m-°C
@Temperature 20.0 - 100 °C
 23.7 - 24.7 µm/m-°C
@Temperature 20.0 - 200 °C
 24.5 - 25.5 µm/m-°C
@Temperature 20.0 - 300 °C
Thermal Conductivity 121.9 W/m-K
@Temperature 30.0 °C
 130.9 W/m-K
@Temperature 100 °C
 144.6 W/m-K
@Temperature 200 °C
 155.7 W/m-K
@Temperature 300 °C
 156.1 W/m-K
@Temperature 400 °C
Melting Point 512 - 659 °C
Solidus 512.3 - 518.3 °C
Liquidus 653.6 - 659.3 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 94 %As Balance
Copper, Cu 5.0 %
Titanium, Ti 1.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Erbslöh Aluminium DISPAL S220 Aluminum Alloy, AlSi35, Condition O
Erbslöh Aluminium DISPAL S691 Aluminum Alloy, AlCu5Ti
Aluminum Weldalite 049-T4
Erbslöh Aluminium DISPAL S690 Aluminum Alloy, AlCu4MgAg, Condition T4
Erbslöh Aluminium DISPAL S690 Aluminum Alloy, AlCu4MgAg, Condition T6

NPEAK08a / 143035

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.