MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Plastics Group Polifil® GFABS-10 10% Glass-Reinforced Acrylonitrile-Butadiene Styrene (ABS)
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), 10% Glass Fiber Filled

Material Notes: Polifil® GFABS series compounds combine the most desirable properties of both components - allowing for enhanced processability and toughness together with the stiffness of glass.

Applications:

  • Firearms
  • Automotive
  • Household appliances

Standard processing techniques are applicable.

Information provided by The Plastics Group.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.10 g/ccASTM D792
Density 1.10 g/ccASTM D792
Filler Content 10 %ASTM D2584
 10.0 %TPG WI
Water Absorption 0.200 %
@Time 86400 sec
ASTM D570
Linear Mold Shrinkage 0.0030 cm/cm
@Thickness 1.59 mm
ASTM D955
 0.00300 in/in
@Thickness 3.17 mm
ASTM D955
Melt Flow 3.00 - 10.0 g/10 min
@Load 3.80 kg,
Temperature 230 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 105ASTM D785
 105ASTM D785
Tensile Strength at Break 9500 psiASTM D638
Tensile Strength 9500 psiASTM D638
Elongation at Break 3.0 %ASTM D638
 3.00 %ASTM D638
Elongation at Yield 2.00 %ASTM D638
Tensile Modulus 670 ksiASTM D638
 670000 psiASTM D638
Flexural Strength 14800 psiASTM D790
 14800 psiASTM D790
Flexural Modulus 600 ksitangent; ASTM D790
 600000 psiTangent; ASTM D790
Compressive Strength 12000 psiASTM D695
Izod Impact, Notched 1.20 ft-lb/inAt 73°F; ASTM D256
 1.20 ft-lb/inASTM D256
Izod Impact, Unnotched 5.60 ft-lb/inAt 73°F; ASTM D256
Gardner Impact 6.00 in-lb
@Thickness 12.7 mm
tup; ASTM D5420
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 3.0
@Frequency 10000 Hz
ASTM D150
Dielectric Strength 450 V/milASTM D149
Dissipation Factor 0.0080
@Frequency 10000 Hz
ASTM D150
Arc Resistance 80 secDry; ASTM D495
 
Thermal PropertiesOriginal ValueComments
CTE, linear 23.0 µm/m-°C
@Temperature 20.0 °C
ASTM D696
Maximum Service Temperature, Air 140 °FContinuous use; UL 746B
Deflection Temperature at 0.46 MPa (66 psi) 210 °FASTM D648
 210 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 208 °FASTM D648
 208 °FASTM D648
Flammability, UL94 HBClass 1/16
Oxygen Index <= 27 %ASTM D2863
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 400 - 420 °F
Middle Barrel Temperature 410 - 430 °F
Front Barrel Temperature 430 - 450 °F
Nozzle Temperature 440 - 450 °F
Melt Temperature 425 - 520 °F
Mold Temperature 100 - 150 °F
Drying Temperature 71.0 °C
@Time 14400 sec
 82.0 °C
@Time 7200 sec
Back Pressure 25.0 - 75.0 psi
Screw Speed 30.0 - 60.0 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Nylon 6, 30% Glass Fiber Filled
Overview of materials for Nylon 6, Unreinforced
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), NCG Fiber Filled
Overview of materials for Polyphenylene Sulfide (PPS) with 40% Glass Fiber Filler
Overview of materials for High Density Polyethylene (HDPE), Glass fiber Filled

PPOLI035 / 56939

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.